Iron-carbon compound for titanium concentrate electric furnace smelting of high titanium slag as well as preparation method and application of iron-carbon compound
By mixing coking acid tar, coking biochemical sludge and coking coal in a specific proportion and distilling the iron-carbon composite prepared, the high cost of reducing agent for smelting high titanium slag for electric furnaces of titanium concentrate is solved, and the problem of difficult solid waste utilization is achieved. Efficient resource reuse and environmental benefits.
Patent Information
- Application Number
- CN202411076421.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The existing titanium concentrate electric furnaces for smelting high-titanium slag are costly and it is difficult to effectively utilize coking acid tar and biochemical sludge, resulting in waste of resources and environmental pollution.
Iron-carbon composites are prepared by mixing coking acid tar, coking biochemical sludge and coking coal in a specific proportion and performing medium-high temperature dry distillation. They are used as a reducing agent for smelting high-titanium slag with titanium concentrate electric furnace to meet the fixed carbon content, ash content and reactivity It is required to achieve the reuse of acid tar and biochemical sludge at the same time.
The prepared iron-carbon composite meets the index requirements for reducing agents for high-titanium slag smelting of titanium concentrate electric furnaces, reduces costs, realizes the resource utilization of solid waste, and has significant environmental protection and economic benefits.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to an iron-carbon composite for smelting high-titanium slag in an electric furnace of titanium concentrate, a preparation method thereof and an application thereof. Background Art
[0002] The reducing agent used in the electric furnace smelting of high titanium slag from titanium concentrate requires high fixed carbon content, low ash content, good reaction activity, and certain strength. The specific requirements are: fixed carbon ≥ 80%, ash ≤ 15%, and volatile matter ≤ 3%. At present, the reducing agents used in the electric furnace smelting of high titanium slag from titanium concentrate are mainly coke and anthracite. Under the current industry background, the price of coke or anthracite remains high, which brings huge cost pressure to the electric furnace smelting of high titanium slag from titanium concentrate.
[0003] The ammonium sulfate and phosphoric acid washing processes in the coking gas purification system will produce a certain amount of acid tar, which is a hazardous waste. The coking wastewater treatment system will produce biochemical sludge, which is also a hazardous waste. Therefore, how to achieve the reuse of acid tar and biochemical sludge is of great significance. Summary of the invention
[0004] The technical problem solved by the present invention is to provide an iron-carbon composite for high-titanium slag smelted in an electric furnace from titanium concentrate, which can not only realize the recycling of coking acid tar and coking biochemical sludge, but also meet the index requirements of reducing agent for high-titanium slag smelted in an electric furnace from titanium concentrate.
[0005] In view of this, the present application provides an iron-carbon composite for smelting high-titanium slag in an electric furnace of titanium concentrate, which is prepared from coking acid tar, coking biochemical sludge and coking coal;
[0006] The content of the coking acid tar is ≤20wt%, the content of the coking biochemical sludge is ≤40wt%, and the content of the coking coal is ≥40wt%.
[0007] Preferably, the mass ratio of the coking acid tar to the coking biochemical sludge is 1:1.5 to 1:3.
[0008] Preferably, the carbon content of the coking acid tar is greater than 80%, the content of iron hydroxide in the coking biochemical sludge is 75-90wt%, and the fixed carbon content of the coking coal is greater than 70wt%.
[0009] Preferably, the moisture content of the coking biochemical sludge is 6-10wt%, and the moisture content of the coking coal is 8-15wt%.
[0010] Preferably, the quality control of the coking coal is as follows: 10%≤dry ash-free volatile matter≤28%, dry basis ash≤8%, particle size≤3mm; the strength of the coke after the single-coal coking reaction is>60%, and the reactivity is<30%.
[0011] The present application also provides a method for preparing the iron-carbon composite for smelting high-titanium slag in an electric furnace of titanium concentrate, comprising the following steps:
[0012] Mixing coking acid tar, coking biochemical sludge and coking coal according to a mass ratio to obtain a mixed material;
[0013] The mixed material is dry-distilled to obtain an iron-carbon composite for high-titanium slag in an electric furnace for refining titanium concentrate.
[0014] Preferably, the moisture content of the mixed material is 9-11%, and the dry ash content is 8-15%.
[0015] Preferably, the starting temperature of the carbonization is 350-450°C, and the final temperature is 700-1100°C.
[0016] Preferably, the heating rate of the dry distillation is 5 to 10° C. / min, and the dry distillation time is 2 to 4 hours.
[0017] The present application also provides a method for smelting high-titanium slag in an electric furnace using titanium concentrate, comprising:
[0018] Mixing titanium concentrate and reducing agent and then smelting;
[0019] The reducing agent is the iron-carbon complex or the iron-carbon complex prepared by the preparation method.
[0020] The present application provides an iron-carbon composite for use in electric furnace smelting of high-titanium slag from titanium concentrate, which is prepared from coking acid tar, coking biochemical sludge and coking coal; the present application utilizes the high carbon content and good adhesion of coking acid tar and the high iron content of coking biochemical sludge in combination with coking coal to prepare the iron-carbon composite, and by adjusting the proportional relationship between the three, the performance characteristics of the three are fully utilized, and ultimately the iron-carbon composite has high reactivity as a reducing agent, meets the index requirements of a reducing agent for use in electric furnace smelting of high-titanium slag from titanium concentrate, and realizes the reuse of coking acid tar and coking biochemical sludge. DETAILED DESCRIPTION
[0021] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0022] In view of the performance requirements of reducing agents for high-titanium slag from electric furnace smelting of titanium concentrate in the prior art and the need to reuse coking acid tar and coking biochemical sludge, the present application provides an iron-carbon composite for high-titanium slag from electric furnace smelting of titanium concentrate, which utilizes solid waste coking acid tar, coking biochemical sludge and coking coal for medium and high temperature carbonization to produce the iron-carbon composite for high-titanium slag from electric furnace smelting of titanium concentrate, thereby realizing the resource utilization of two solid wastes, coking acid tar and coking biochemical sludge. At the same time, the prepared iron-carbon composite meets the index requirements of reducing agents for high-titanium slag from electric furnace smelting of titanium concentrate. Specifically, an embodiment of the present invention discloses an iron-carbon composite for high-titanium slag from electric furnace smelting of titanium concentrate, which is prepared from coking acid tar, coking biochemical sludge and coking coal;
[0023] The content of the coking acid tar is ≤20wt%, the content of the coking biochemical sludge is ≤40wt%, and the content of the coking coal is ≥40wt%.
[0024] In the raw materials for preparing the iron-carbon composite, the coking acid tar has a high carbon content and good adhesion. In the present application, the carbon content of the coking acid tar is greater than 80%, specifically, the carbon content of the coking acid tar is 83.5-88%, and the carbon content in the coking acid tar is required to meet the index requirements of the prepared iron-carbon composite as a reducing agent. The content of the coking acid tar is ≤20wt%, specifically, the content of the coking acid tar is 2-18wt%, more specifically, the content of the coking acid tar is 5-15wt%, and more specifically, the content of the coking acid tar is 8-10wt%.
[0025] The coking biochemical sludge has a high iron content, and its main component is ferric hydroxide to provide an iron source; the coking acid tar provides carbon and can also react with the coking biochemical sludge to provide an iron source for a reducing agent used in the electric furnace smelting of high-titanium slag in titanium concentrate. The content of the coking biochemical sludge is ≤40wt%, specifically, the content of the coking biochemical sludge is 10-38wt%, more specifically, the content of the coking biochemical sludge is 15-35wt%, and more specifically, the content of the coking biochemical sludge is 20-25wt%. Further, the mass ratio of the coking acid tar to the coking biochemical sludge is 1:1.5 to 1:3, specifically, the mass ratio of the coking acid tar to the coking biochemical sludge is 1:1.6 to 1:2.6, more specifically, the mass ratio of the coking acid tar to the coking biochemical sludge is 1:1.8 to 1:2.5, more specifically, the mass ratio of the coking acid tar to the coking biochemical sludge is 1:2 to 1:2.3. In the present application, the content of iron hydroxide in the coking biochemical sludge is 75 to 90 wt%, specifically, the content of iron hydroxide is 78 to 88 wt%, more specifically, the content of iron hydroxide is 80 to 85 wt%. The moisture content of the coking biochemical sludge is 6 to 10 wt%, specifically, the moisture content of the coking biochemical sludge is 7 to 9 wt%; too high a moisture content of the coking biochemical sludge will affect its actual addition amount, thereby affecting the performance of the iron-carbon composite.
[0026] The coking coal is a main component of the iron-carbon composite, and its content is ≥40wt%, specifically, the content of the coking coal is 42-75wt%, more specifically, the content of the coking coal is 45-70wt%, more specifically, the content of the coking coal is 50-60wt%. The fixed carbon content of the coking coal is greater than 70wt%, the moisture content of the coking coal is 8-15wt%, specifically, the fixed carbon content of the coking coal is 72-85%wt%, and the moisture content of the coking coal is 10-13wt%. Furthermore, the quality control of the coking coal is as follows: 10%≤dry ash-free volatile matter≤28%, dry ash content≤8%, particle size≤3mm; the strength of the coke after the reaction of single-coal coking is>60%, and the reactivity is<30%; Specifically, the quality control of the coking coal is as follows: 12%≤dry ash-free volatile matter≤20%, dry ash content is 7.0-7.9%, and particle size≤3mm; the strength of the coke after the reaction of single-coal coking is 63-72.5%, and the reactivity is 19.6-28%.
[0027] The above three kinds of raw materials need to maintain a specific ratio of the coking acid tar and the coking biochemical sludge due to their components and reaction characteristics. The mixture of coking coal, coking acid tar and coking biochemical sludge has a certain coking property, so that the mixture can be bonded into blocks under high-temperature dry distillation isolated from air, so that it has a certain strength.
[0028] Furthermore, the present application also provides a method for preparing an iron-carbon composite for smelting high-titanium slag in an electric furnace of titanium concentrate, comprising the following steps:
[0029] Mixing coking acid tar, coking biochemical sludge and coking coal according to a mass ratio to obtain a mixed material;
[0030] The mixed material is dry-distilled to obtain an iron-carbon composite for high-titanium slag in an electric furnace for refining titanium concentrate.
[0031] In the process of preparing the iron-carbon composite, the present application first mixes coking acid tar, coking biochemical sludge and coking coal to obtain a mixed material; the mixing method is carried out in a manner well known to those skilled in the art, and the present application does not impose any particular restrictions on this. The moisture content of the mixed material is 9-11%, and the dry basis ash content is 8-15%, so as to meet the index requirements of the iron-carbon composite as a catalyst.
[0032] The present application then performs dry distillation on the mixture to obtain an iron-carbon composite for high-titanium slag for electric furnace refining of titanium concentrate; the starting temperature of the dry distillation is 350-450°C, and the final temperature is 700-1100°C. Specifically, the starting temperature of the dry distillation is 400°C, and the final temperature is 800-1000°C. The heating rate of the dry distillation is 5-10°C / min, and the dry distillation time is 2-4h. Specifically, the heating rate of the dry distillation is 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, and the dry distillation time is 2h, 3h or 4h.
[0033] In a specific embodiment, the preparation method of the iron-carbon composite is specifically as follows:
[0034] 1) Coking acid tar, coking biochemical sludge and coking coal are uniformly mixed according to the mass ratio, and the mixed materials are added into a retort that has been heated to 400° C. (such as coke ovens of different specifications such as 2kg, 20kg, 40kg or crucibles of different specifications such as 100g, 200g, 500g) for medium-high temperature retort, and the temperature needs to be kept constant for 2 to 4 hours after reaching the final retort temperature; the final retort temperature is 700° C. to 1100° C.; the retort temperature is increased at a rate of 10° C. / min from 0 to 400° C., and the temperature increase rate from 400° C. to the final retort temperature is 15° C. / min;
[0035] 2) The retort is taken out from the heating furnace and allowed to cool naturally to room temperature without opening the retort cover (with holes for gas discharge) to obtain an iron-carbon composite for high-titanium slag in an electric furnace for smelting titanium concentrate.
[0036] The present application also provides a method for smelting high-titanium slag in an electric furnace using titanium concentrate, comprising:
[0037] Mixing titanium concentrate and reducing agent and then smelting;
[0038] The reducing agent is the iron-carbon complex described in the above scheme.
[0039] The acid tar produced by the coke oven gas purification system of the coking enterprise has high carbon content and high cohesiveness, but due to its high acid content, it is a hazardous waste; the biochemical sludge produced by the coking wastewater treatment system is mainly ferric hydroxide, which is also a hazardous waste. The present application makes full use of the acidity and cohesiveness of the acid tar and the alkalinity and iron-containing biochemical sludge, and mixes them with coking coal and then performs medium and high temperature dry distillation, so that the acidity of the coking acid tar and the alkalinity of the coking biochemical sludge are neutralized. At the same time, due to the iron-containing nature of the coking biochemical sludge and the strong cohesiveness of the coking acid tar, these iron-carbon composites produced after medium and high temperature dry distillation mixed with coking coal not only have a high fixed carbon content, but also have a certain strength and high reactivity (reducibility), meet the requirements of iron-carbon composites for high-titanium slag smelting in titanium concentrate electric furnace, and realize the resource utilization of two solid wastes, coking acid tar and coking biochemical sludge, with significant environmental and economic benefits.
[0040] In order to further understand the present invention, the preparation method of the iron-carbon composite for high-titanium slag smelting in electric furnace of titanium concentrate provided by the present invention is described in detail below in conjunction with examples, and the protection scope of the present invention is not limited by the following examples.
[0041] Example 1
[0042] Take 10 parts of coking acid tar, 20 parts of coking biochemical sludge, and 70 parts of coking coal, mix them evenly to obtain a mixed material, and the moisture content of the mixed material is controlled to be 10%;
[0043] Among them, the carbon content of coking acid tar is 83.5%; the content of iron hydroxide in coking biochemical sludge is 85%, and the moisture content is 6% (dried to less than 10%); the fixed carbon content of coking coal is 72%, the moisture content is 8%, the content of dry ash-free volatile matter is 20%, the content of dry ash is 7.9%, the particle size is ≤3mm, and the strength of single-coal coke after reaction is 72.5%, and the reactivity is 19.6%;
[0044] The mixed material is added into the retort, and the retort is placed into a heating furnace heated to 400°C, and the temperature is increased at a heating rate of 5°C / min, and the final retort temperature is set to 1000°C. After reaching the final retort temperature, the temperature is kept constant for 3 hours;
[0045] The retort is taken out from the heating furnace and naturally cooled to room temperature without opening the cover to obtain the iron-carbon composite (reducing agent) for high-titanium slag smelting in an electric furnace of titanium concentrate.
[0046] The index detection results of the iron-carbon composite prepared in this example are shown in Table 1.
[0047] Example 2
[0048] Take 15 parts of coking acid tar, 25 parts of coking biochemical sludge, and 60 parts of coking coal, mix them evenly to obtain a mixed material, and the moisture content of the mixed material is controlled to be 10%;
[0049] Among them, the carbon content of coking acid tar is 83.5%; the content of iron hydroxide in coking biochemical sludge is 85%, and the moisture content is 6%; the fixed carbon content of coking coal is 72%, the moisture content is 8%, the content of dry ash-free volatile matter is 20%, the content of dry ash is 7.9%, the particle size is ≤3mm, the strength of single coal coking coke after reaction is 72.5%, and the reactivity is 19.6%;
[0050] The mixed material is added into the retort, and the retort is placed into a heating furnace heated to 400°C, and the temperature is increased at a heating rate of 5°C / min, and the final retort temperature is set to 1000°C. After reaching the final retort temperature, the temperature is kept constant for 3 hours;
[0051] The retort is taken out from the heating furnace and naturally cooled to room temperature without opening the cover to obtain the iron-carbon composite (reducing agent) for high-titanium slag smelting in an electric furnace of titanium concentrate.
[0052] The index detection results of the iron-carbon composite prepared in this example are shown in Table 1.
[0053] Example 3
[0054] Take 20 parts of coking acid tar, 40 parts of coking biochemical sludge, and 40 parts of coking coal, mix them evenly to obtain a mixed material, and the moisture content of the mixed material is controlled to be 10%;
[0055] Among them, the carbon content of coking acid tar is 83.5%; the content of iron hydroxide in coking biochemical sludge is 85%, and the moisture content is 6%; the fixed carbon content of coking coal is 72%, the moisture content is 8%, the content of dry ash-free volatile matter is 20%, the content of dry ash is 7.9%, the particle size is ≤3mm, the strength of single coal coking coke after reaction is 72.5%, and the reactivity is 19.6%;
[0056] The mixed material is added into the retort, and the retort is placed into a heating furnace heated to 400°C, and the temperature is increased at a heating rate of 5°C / min, and the final retort temperature is set to 1000°C. After reaching the final retort temperature, the temperature is kept constant for 3 hours;
[0057] The retort is taken out from the heating furnace and naturally cooled to room temperature without opening the cover to obtain the iron-carbon composite (reducing agent) for high-titanium slag smelting in an electric furnace of titanium concentrate.
[0058] The index detection results of the iron-carbon composite prepared in this example are shown in Table 1.
[0059] Table 1 Test results of iron-carbon composite (reducing agent) for high-titanium slag smelted in electric furnace of titanium concentrate prepared in Example
[0060] Example Fixed carbon / % Ash / % Volatile matter / % Reactivity / % Strength after reaction / % Example 1 87.2 9.8 1.2 35.2 52.7 Example 2 85.5 12.6 1.3 39.7 48.3 Example 3 81.3 14.8 1.2 48.2 37.6
[0061] From the above test results, it can be seen that the iron-carbon composites prepared in the above examples can meet the index requirements of reducing agents for high-titanium slag smelting in electric furnaces of titanium concentrate.
[0062] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0063] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An iron-carbon composite for smelting high-titanium slag in an electric furnace of titanium concentrate, prepared from coking acid tar, coking biochemical sludge and coking coal; The content of the coking acid tar is ≤20wt%, the content of the coking biochemical sludge is ≤40wt%, and the content of the coking coal is ≥40wt%.
2. The iron-carbon composite according to claim 1, It is characterized in that The mass ratio of the coking acid tar to the coking biochemical sludge is 1:1.5 to 1:
3.
3. The iron-carbon composite according to claim 1, It is characterized in that The carbon content of the coking acid tar is greater than 80%, the content of iron hydroxide in the coking biochemical sludge is 75-90wt%, and the fixed carbon content of the coking coal is greater than 70wt%.
4. The iron-carbon composite according to claim 1, It is characterized in that The moisture content of the coking biochemical sludge is 6-10wt%, and the moisture content of the coking coal is 8-15wt%.
5. The iron-carbon composite according to claim 1, It is characterized in that The quality control of the coking coal is as follows: 10%≤dry ash-free volatile matter≤28%, dry ash≤8%, particle size≤3mm; the strength of the coke after the single-coal coking reaction is>60%, and the reactivity is <30%.
6. The method for preparing the iron-carbon composite for smelting high-titanium slag in an electric furnace of titanium concentrate according to claim 1, The following steps are involved: Mixing coking acid tar, coking biochemical sludge and coking coal according to a mass ratio to obtain a mixed material; The mixed material is dry-distilled to obtain an iron-carbon composite for high-titanium slag in an electric furnace for refining titanium concentrate.
7. The preparation method according to claim 6, It is characterized in that The moisture content of the mixed material is 9-11%, and the dry ash content is 8-15%.
8. The preparation method according to claim 6, It is characterized in that The starting temperature of the carbonization is 350-450°C, and the final temperature is 700-1100°C.
9. The preparation method according to claim 8, It is characterized in that The heating rate of the dry distillation is 5 to 10° C. / min, and the time of the dry distillation is 2 to 4 hours.
10. A method for smelting high-titanium slag in an electric furnace with titanium concentrate, include: Mixing titanium concentrate and reducing agent and then smelting; The reducing agent is the iron-carbon composite according to any one of claims 1 to 5 or the iron-carbon composite prepared by the preparation method according to any one of claims 6 to 9.
Citation Information
Patent Citations
Iron-carbon micro-electrolysis filler and preparation method thereof
CN103274503A
Ferrous coke composite pellet containing tar residues and production method thereof
CN104419825A
Method for producing iron coke composite furnace burden by using steel rolling sludge
CN109957431A
Method for preparing ironmaking fuel from carbon-containing waste
CN117106502A
High reactivity and high strength coke for blast furnace and method of producing the same
KR101657402B1