Method for recovering and extracting lithium from retired lithium ion battery

Lithium carbonate precipitation is generated by reacting lithium, graphite and oxygen with contact with high pressure water mist at high temperature, which solves the complex and high cost of recycling process of negative electrode materials for retired lithium-ion batteries, and achieves efficient and low-cost lithium-ion extraction and Improved purity.

CN118979153APending Publication Date: 2024-11-19ZHEJIANG BAIMA LAKE LABORATORY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410785316.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The wet recovery process of existing retired lithium-ion battery negative electrode materials is complex and has high cost, the yield of lithium carbonate is low, and the purity is difficult to meet the battery level requirements.

Method used

By reacting lithium, graphite and oxygen at high temperature, carbonic acid and lithium hydroxide undergo acid-base neutralization reaction, forming lithium carbonate precipitation, improving the efficiency and purity of lithium recovery and extraction.

Benefits of technology

It has achieved efficient lithium extraction of lithium-ion negative electrode materials for lithium-ion batteries, with simple process and low cost, high purity of lithium carbonate and high efficiency, and solved the problems of cumbersome process and high cost in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979153A_ABST
    Figure CN118979153A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of recycling of decommissioned lithium ion batteries, and discloses a method for recycling and extracting lithium from decommissioned lithium ion batteries, which comprises the following steps: S1, after the decommissioned lithium ion batteries are fully charged, dissecting the decommissioned lithium ion batteries, taking out negative plates, and then crushing the decommissioned lithium ion batteries in a glove box or a dew-point room; s2, transferring the crushed negative electrode plate into a reaction kettle filled with inert atmosphere protection, then introducing high-purity oxygen, and heating for reaction; s3, after the reaction is completed, reducing the temperature to normal temperature, and introducing high-pressure water mist; and S4, sieving, washing, centrifuging and drying the solid obtained in S3 to obtain a lithium carbonate product. Carbon dioxide is generated through high-temperature graphite oxide, carbon dioxide does not need to be introduced from the outside, the solubility of carbon dioxide in water is improved through high-pressure water mist, the reaction speed is increased, the lithium extraction efficiency and purity are improved, and the cost is lower.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of recycling retired lithium-ion batteries, and in particular to a method for recycling and extracting lithium from retired lithium-ion batteries. Background Art

[0002] With the continuous promotion of new energy vehicles in my country in recent years, the number of electric vehicles has continued to increase, and the installed capacity of power batteries has also increased accordingly. Since the average life of power batteries for new energy vehicles is generally around 5 to 8 years, the power batteries have entered a large-scale retirement stage since 2018. At the same time, facing the multiple pressures of tight metal resources such as nickel, cobalt, and lithium and rising costs, the scale of the retired power battery recycling market has expanded rapidly.

[0003] In the future, a more effective cooperation mechanism will be established between automobile manufacturers, battery manufacturers and other companies. The main participants in the power battery recycling market, such as power battery or material manufacturers, third-party professional recycling companies, industry alliances, etc., will work closely with automobile manufacturers to achieve the rapid return of used batteries to the factory. Therefore, the industry's demand for recycling efficiency and cost will increase significantly.

[0004] Power disassembly and recycling refers to the centralized recycling of scrapped power batteries, the recovery of nickel, cobalt, manganese, copper, aluminum, lithium and other metals in the batteries through process technology, and then the recycling of these materials. At present, the recycling processes of power battery electrolytic materials mainly include physical recycling, pyrometallurgical recycling and wet recycling. The core difference between the three methods lies in the different processes of extracting metals. Taking wet recycling as an example, wet recycling is to disassemble and pre-treat the waste batteries and dissolve them in acid and alkali solutions to extract some valuable metal elements, and then extract the remaining valuable metals through ion exchange and electrodeposition. It mainly includes three methods: chemical precipitation, solvent extraction and ion exchange. The core process of the wet method is to add chemical reagents to the battery powder for leaching and extraction. The advantages are low equipment and operation requirements, multiple chemical reaction selectivity, high product purity, and high efficiency for the recovery of heavy metal substances in batteries; the disadvantages are long process flow, corrosive solvents involved in the recycling process, and problems such as waste liquid pollution.

[0005] For the recycling mode, the positive electrode has a high value and is the main recycling focus at present. For the recycling of relatively low-value main materials such as negative electrodes, electrolytes and diaphragms, the industrialization process is advancing slowly. After the positive electrode materials of many retired or scrapped lithium-ion batteries are recycled and reused, the negative electrode materials are mostly disposed of by landfill or incineration. In the wet recovery of existing negative electrode materials, acid solution is often used to dissolve lithium elements and their compounds. During the recovery process, the alkaline solution compounds generated by lithium and its compounds require a large amount of acid solution. Subsequently, a large amount of alkaline solution is used to neutralize the alkaline solution containing lithium and other metal ions to obtain lithium carbonate precipitation. At the same time, the presence of other valuable metal ions will affect the purity of lithium carbonate. The patent with application number 202210096575.2 discloses a method for recycling the negative electrode of waste lithium-ion batteries. The discharged negative electrode plate is immersed in water to react with lithium to generate lithium hydroxide, and carbon dioxide gas or carbonate is introduced to react with lithium hydroxide to generate lithium carbonate precipitation to achieve the purpose of lithium extraction. The disadvantages of this technology are: 1. This technology uses the negative electrode plate after emptying to recover the lithium source, graphite and copper current collector. At this time, there is a lack of sufficient active lithium in the negative electrode plate, and there are only some lithium and lithium compounds on the surface of the plate and a small amount of lithium source in the graphite; 2. Carbon dioxide has low solubility in water and can only generate limited carbonic acid, and the reaction conditions required for the replacement reaction of lithium and sodium are harsh (generally temperature>200℃, pressure>2.0MPa); 3. A large amount of acid and alkali are still consumed in the process of purifying lithium carbonate. Therefore, the technical process disclosed in this invention is cumbersome, long, and costly, and the recovery rate of lithium carbonate is low, and the purity is difficult to meet the requirements of battery-grade lithium carbonate. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a method for recovering and extracting lithium from retired lithium-ion batteries. Lithium and graphite are oxidized by reaction with oxygen at high temperature and then fully contacted with injected high-pressure water mist particles. The generated carbonic acid reacts with lithium hydroxide to produce lithium carbonate precipitate by acid-base neutralization reaction, thereby improving the efficiency and purity of lithium recovery.

[0007] The purpose of the present invention is achieved through the following technical solution: The present invention provides a method for recovering and extracting lithium from retired lithium-ion batteries, comprising the following steps: S1: After the retired lithium-ion battery is fully charged, the negative electrode sheet is dissected out and crushed. This process is carried out in a glove box or dew point room; S2: The crushed negative electrode sheet is transferred to a reactor protected by an inert atmosphere, and then high-purity oxygen is introduced and the temperature is raised for reaction; S3: After the reaction is completed, the temperature is lowered to room temperature and high-pressure water mist is introduced; S4: The solid obtained in S3 is sieved, washed, centrifuged and dried to obtain a lithium carbonate product.

[0008] The reaction equation of the above process is as follows: 2Li+O 2 →2Li 2 O C+O 2 →CO 2 Li 2 O+H 2 O→2LiOH CO 2 +H 2 O + 2LiOH → Li 2 CO 3 +2H 2 O The negative electrode of commercial lithium-ion batteries mostly uses layered graphite materials. When the battery is fully charged, lithium ions are embedded in the graphite layer structure. The lithium-embedded negative electrode sheets are recycled, crushed, processed, etc. to obtain reusable high-purity lithium carbonate raw materials. There are few types of elements in the negative electrode sheet and the separation is simple. The present invention uses a one-step method to quickly extract lithium from the lithium-embedded negative electrode sheet. The method has a simple lithium extraction process, a short process, low cost and high efficiency, and the obtained lithium carbonate has high purity.

[0009] The present invention provides a one-step lithium extraction method for retired lithium-ion batteries. The remaining available lithium source in the battery is transferred to the negative electrode by charging. The lithium ions are stored in the graphite layered structure connected by van der Waals forces. The metal elements contained in the negative electrode are mainly lithium metal, which is of few types and easy to extract. The technology is that lithium and graphite react with oxygen at high temperature to oxidize and then fully contact with the injected high-pressure water mist particles. The generated carbonic acid reacts with lithium hydroxide to produce lithium carbonate precipitate by acid-base neutralization reaction. The lithium extraction method provided by the invention is low-cost, high-efficiency, simple process and high-purity.

[0010] Preferably, the negative electrode sheet uses graphite as the negative electrode active material.

[0011] Preferably, the relative humidity of the dew point in the dew point room in S1 is controlled to be ≤-50°C; the oxygen content in the glove box is ≤1ppm, and the water content is ≤1ppm.

[0012] Preferably, the inert atmosphere in S2 is an argon atmosphere with a purity of ≥99.9%.

[0013] Preferably, the high-purity oxygen in S2 has a purity of ≥99.9%.

[0014] Preferably, the temperature of the heating in S2 is 500-1500°C, and the reaction time is 30min-5h. More preferably, the temperature of the heating is 700-1200°C, and the reaction time is 3-5h.

[0015] Under the conditions specified by these parameters, oxygen can fully react with the graphite negative electrode and generate sufficient carbon dioxide gas, which helps the subsequent reactions.

[0016] Preferably, the pressure of the high-pressure water mist in S3 is P≥1MPa, and the cumulative distribution of droplets on a plane 1m away from the nozzle is Dv0.99<1000μm.

[0017] The high-pressure water mist can increase the solubility of carbon dioxide in water, and the fine particles of the water mist are in full contact with the carbon dioxide generated by graphite oxidation, increasing the reaction rate and improving the efficiency of lithium extraction.

[0018] Preferably, the high-pressure water mist is introduced for a time of 20 minutes to 3 hours in S3. More preferably, the high-pressure water mist is introduced for a time of 1 to 3 hours.

[0019] Preferably, in S3, the high-pressure water mist process is introduced and circulating cooling water is used for cooling to keep the solution temperature below 30°C.

[0020] Preferably, the mesh size of the sieve used for screening in S4 is ≤0.5 μm.

[0021] Preferably, the washing in S4 is performed by water washing, and the mass ratio of pure water to precipitate is ≥5:1.

[0022] Preferably, the centrifugal speed in S4 is not less than 1000 rpm.

[0023] Preferably, the drying temperature in S4 is not less than 100°C.

[0024] Compared with the prior art, the present invention has the following beneficial effects: (1) There are many types of elements in the positive electrode material, which is difficult to purify, with complex processes and high costs. The present invention charges retired lithium-ion batteries to fully transfer the remaining reversible lithium source to the negative electrode graphite layer, which is beneficial to the efficient extraction of lithium, greatly improves the yield, and has a high purity and lower cost.

[0025] (2) The present invention creatively utilizes high-temperature oxidation of graphite carbon to generate carbon dioxide. Carbon dioxide does not need to be introduced from the outside. When graphite is oxidized at high temperature, the lithium embedded in the graphite layered structure can also react fully. This method can maximize the separation and purification of lithium sources.

[0026] (3) The solubility of carbon dioxide gas in water increases with decreasing temperature and increasing pressure. The present invention utilizes high-pressure water mist to increase the solubility of carbon dioxide in water. On the other hand, the fine particles of the water mist are in full contact with the carbon dioxide generated by graphite oxidation, thereby increasing the reaction speed and improving efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The figure is a schematic diagram of the process flow of recovering and extracting lithium according to the present invention.

[0028] The reference numerals in the drawings are: crusher 1, conveyor belt 2, reactor 3, high-pressure water mist 4, sieve 5, dryer 6. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto: A schematic diagram of a process flow for recycling and extracting lithium from retired lithium-ion batteries is shown in Figure 1 As shown, it includes a pulverizer 1, a reactor 3 and a dryer 6 which are sequentially connected via a conveyor belt 2. High-pressure water mist 4 is introduced into the upper part of the reactor 3, and the bottom solids are separated from the lower part of the reactor 3 by screening 5 for subsequent treatment.

[0030] The process specifically includes the following steps: S1: After the retired lithium-ion battery is fully charged, it is dissected in a glove box or a dew point room. After the lithium-intercalated negative electrode sheet is taken out, the negative electrode sheet is transferred to a pulverizer 1 and pulverized, and the weight of the pulverized negative electrode sheet is recorded.

[0031] S2: The crushed negative electrode sheet is transferred to a reactor 3 protected by an inert atmosphere through a conveyor belt 2, and then high-purity oxygen (purity ≥ 99.9%) is introduced, the temperature is raised to 500-1500°C, and the reaction is carried out for 30 minutes to 5 hours; after the reaction is completed, the reaction is stopped, the temperature is lowered to room temperature, the solids at the bottom of the reactor 3 including the copper current collector and some unreacted solids are separated, and the solid weight is recorded.

[0032] S3: introduce high-pressure water mist 4 (pressure P of high-pressure water mist 4 ≥ 1MPa, cumulative distribution of droplets on a plane 1m away from the nozzle Dv0.99 < 1000μm), and continue to spray high-pressure water mist 4 into the reactor 3 after the temperature drops to room temperature (the water used for the water mist here can be deionized water, high-purity distilled water, etc.), and stop after the water in the reactor 3 completely immerses the solids. The introduction time of high-pressure water mist 4 is 20min to 3h, and the solids at the bottom of the reactor 3 are sieved through a filter with a pore size of ≤ 0.5μm 5, and the weight of the initial lithium carbonate obtained is recorded. Since the reaction will generate a lot of heat, in order to prevent the lithium carbonate from sticking to the wall and causing low yield and purity, it is necessary to cool the solution by circulating cooling water to keep the solution temperature below 30°C.

[0033] S4: Wash the solid obtained in S3 with pure water, adding pure water and precipitate in a mass ratio of ≥5:1, the washing temperature is 80-90°C, and the time is 1-3h; then centrifuge, the centrifugal speed is not less than 1000rpm, and then transfer to the dryer 6 through the conveyor belt 2, and dry it in the dryer 6 at a temperature not less than 100°C to obtain a high-purity lithium carbonate product, and record its weight.

[0034] Example 1 The specific steps are as follows: S1: Battery disassembly and electrode crushing. Disassemble the retired lithium battery module into single cells, charge each single cell separately, and charge to the acceptable voltage upper limit (full charge state) according to the attenuation of different single cells. In this embodiment, the lithium iron phosphate single cell is charged at constant current to 3.65V and then converted to constant voltage charging with 0.05C as the cutoff condition. After the single cell is fully charged, it is transferred to the dew point room for disassembly, and the negative electrode plate in the lithium embedded state is taken out. The negative electrode plate is transferred to the crusher for crushing, and the weight of the crushed negative electrode plate is 10kg.

[0035] S2: Oxidation of graphite carbon and lithium. The crushed negative electrode sheet is transferred to the first reactor via a conveyor belt. The reactor has a volume of 50L. High-purity argon (≥99.9%) is introduced into the reactor in advance to expel the air. Then high-purity oxygen (≥99.9%) is introduced, and the temperature in the reactor rises to 1000°C and maintained. The reaction is stopped after continuous introduction of high-purity oxygen for 5 hours. The solids separated from the bottom of the reactor include the copper current collector and some unreacted solids, weighing 3kg.

[0036] S3: Pass high-pressure water mist. After the temperature drops to room temperature, continue to spray high-pressure water mist (deionized water, pressure of high-pressure water mist P = 1MPa, cumulative distribution of droplets Dv0.99 < 1000μm on a plane 1m away from the nozzle) into the reactor. Stop after the water in the reactor completely immerses the solids. The high-pressure water mist is passed for 2h. The solids at the bottom of the reactor are passed through a sieve with a pore size of 0.5μm. The weight of the initial lithium carbonate obtained is 5kg. Since the reaction will generate a lot of heat, in order to prevent the lithium carbonate from sticking to the wall and causing low yield and purity, it is necessary to cool the solution by circulating cooling water to keep the solution temperature below 30°C.

[0037] S4: Washing, centrifugation and drying to obtain high-purity lithium carbonate product. The solid obtained in S3 is washed with pure water for 20 minutes at a temperature of 100°C. The mass of pure water added is 20 kg. The washed lithium carbonate is centrifuged and then dried at 100°C to finally obtain 4.7 kg of high-purity lithium carbonate product.

[0038] Example 2 The specific steps are as follows: S1: Battery disassembly and electrode crushing. Disassemble the retired lithium battery module into single cells, charge each single cell separately, and charge to the acceptable voltage upper limit (full charge state) according to the attenuation of different single cells. In this embodiment, the lithium iron phosphate single cell is charged at constant current to 3.6V and then converted to constant voltage charging with 0.1C as the cutoff condition. After the single cell is fully charged, it is transferred to the dew point room for disassembly, and the negative electrode plate in the lithium embedded state is taken out. The negative electrode plate is transferred to the crusher for crushing. The weight of the crushed negative electrode plate is 8kg.

[0039] S2: Oxidation of graphite carbon and lithium. The crushed negative electrode sheet is transferred to the first reactor via a conveyor belt. The reactor has a volume of 30L. High-purity argon (≥99.9%) is introduced into the reactor in advance to expel the air. Then high-purity oxygen (≥99.9%) is introduced, and the temperature in the reactor rises to 750°C and maintained. The reaction is stopped after continuous introduction of high-purity oxygen for 3 hours. The solids separated from the bottom of the reactor include the copper current collector and some unreacted solids, weighing 2.7kg.

[0040] S3: Pass high-pressure water mist. After the temperature drops to room temperature, continue to spray high-pressure water mist (deionized water, pressure of high-pressure water mist P = 1MPa, cumulative distribution of droplets Dv0.99 < 1000μm on a plane 1m away from the nozzle) into the reactor. Stop after the water in the reactor completely immerses the solids. The high-pressure water mist is passed for 2h. The solids at the bottom of the reactor are filtered through a filter with a pore size of 0.1μm. The weight of the obtained lithium carbonate is 3.9kg. Since the reaction will generate a lot of heat, in order to prevent the lithium carbonate from sticking to the wall and causing low yield and purity, it is necessary to cool the solution by circulating cooling water to keep the temperature below 30°C.

[0041] S4: Washing, centrifugation and drying to obtain high-purity lithium carbonate product. The solid obtained in S3 is washed with pure water solution for 40 minutes at 90°C, and the mass of pure water added is 15kg. The washed lithium carbonate is centrifuged and then dried at 130°C to finally obtain 3.5kg of high-purity lithium carbonate product.

[0042] Example 3 The specific steps are as follows: S1: Battery disassembly and electrode crushing. Disassemble the retired lithium battery module into single cells, charge each single cell separately, and charge to the acceptable voltage upper limit (full charge state) according to the attenuation of different single cells. In this embodiment, the lithium iron phosphate single cell is charged at a constant current to 3.65V before charging. After the single cell is fully charged, it is transferred to the dew point room for disassembly, and the negative electrode plate in the lithium embedded state is taken out. The negative electrode plate is transferred to the crusher for crushing. The weight of the crushed negative electrode plate is 15kg.

[0043] S2: Oxidation of graphite carbon and lithium. The crushed negative electrode sheet is transferred to the first reactor via a conveyor belt. The reactor has a volume of 40L. High-purity argon (≥99.9%) is introduced into the reactor in advance to expel the air. Then high-purity oxygen (≥99.9%) is introduced, and the temperature in the reactor rises to 800°C and maintained. The reaction is stopped after continuous introduction of high-purity oxygen for 2 hours. The solids at the bottom of the reactor are separated, including the copper current collector and some unreacted solids, weighing 5kg.

[0044] S3: Pass high-pressure water mist. After the temperature drops to room temperature, continue to spray high-pressure water mist (deionized water, pressure of high-pressure water mist P = 1MPa, cumulative distribution of droplets Dv0.99 < 1000μm on a plane 1m away from the nozzle) into the reactor. Stop after the water in the reactor completely immerses the solids. The high-pressure water mist is passed for 1h. The solids at the bottom of the reactor are filtered through a filter with a pore size of 0.2μm. The weight of the obtained lithium carbonate initial product is 6.6Kg. Since the reaction will generate a lot of heat, in order to prevent the lithium carbonate from sticking to the wall and causing low yield and purity, it is necessary to cool the solution by circulating cooling water to keep the solution temperature below 30°C.

[0045] S4: Washing, centrifugation and drying to obtain high-purity lithium carbonate product. The solid obtained in S3 is washed with pure water solution for 1 hour at 80°C, and the mass of pure water added is 30kg. The washed lithium carbonate is centrifuged and then dried at 120°C to finally obtain 6.4kg of high-purity lithium carbonate product.

[0046] Comparative Example 1 S1: Take the negative electrode sheet obtained by disassembling the used lithium-ion battery after discharge, break it into 20 pieces of 10cm*10cm in size, put it into a 500mL beaker, inject 350mL of deionized water into it, soak it in water at room temperature, ultrasonicate and mechanically stir it for 0.5h, after the negative electrode powder is completely separated from the collector, filter and take out the collector for recycling, and obtain a Cu collector with a mass of 14.20g. Centrifuge the obtained negative electrode powder mixture to obtain a supernatant containing a binder and a thickener and 28.46g of carbon powder sludge, respectively, heat the supernatant and concentrate it, and pass carbon dioxide gas at the same time, and cool it down to obtain a crude Li 2 CO 3 crystals, the obtained crude Li 2 CO 3 The crystals are configured into a solution and then recrystallized to obtain battery-grade Li 2 CO 3 The mass is 2.76g.

[0047] S2: The 28.46 g of carbon powder sludge obtained in the above step was subjected to acid leaching treatment, added to 500 mL of 0.5 mol / L oxalic acid solution, and mechanically stirred. The reaction temperature was 50°C and the reaction time was 1 h. The mixed solution was then centrifuged to obtain the supernatant after acid leaching and the graphite slurry to be modified. The graphite slurry to be modified was washed and dried to obtain 27.43 g of graphite to be modified.

[0048] S3: Add 6 wt% phenolic resin to the acid-leached graphite to be modified, then ball-mill to obtain a mixed slurry, and then blow dry it at 150°C for 3 h. Place the obtained modified graphite precursor in a crucible under N 2 The calcination was carried out under atmosphere with a heating rate of 5°C / min to 850°C and kept for 4h to obtain modified graphite.

[0049] S4: Remove other metal impurities from the supernatant after acid leaching in S2, add NaOH to adjust the pH to between 7 and 8, then introduce carbon dioxide into the solution, and repeat the lithium extraction operation to obtain battery-grade Li 2 CO 3 The mass is 1.49 g. The obtained battery-grade Li 2 CO 3 The total mass is (2.76+1.49)g.

[0050] Comparative Example 2 S1: Take the negative electrode sheet obtained by disassembling the discharged waste lithium-ion battery, break it into 20 pieces of 10cm*10cm in size, put it into a 500mL beaker, inject 350mL of deionized water into it, heat it to 45℃, ultrasonically and mechanically stir it for 0.5h, and after the negative electrode powder and the current collector are completely separated, filter and take out the current collector for recycling. Centrifuge the obtained negative electrode powder mixture to obtain 29.01g of supernatant containing binder and thickener and carbon powder sludge respectively, heat the supernatant and concentrate it, and introduce carbon dioxide gas at the same time, and cool it down to obtain crude Li 2 CO 3 crystals, the obtained crude Li 2 CO 3 The crystals are configured into a solution and then recrystallized to obtain battery-grade Li 2 CO 3 The mass is 2.73g.

[0051] S2: The 29.01 carbon powder sludge obtained in the above step was washed and then subjected to acid leaching treatment, added to 500mL of a 0.5mol / L malic acid solution, and mechanically stirred. The reaction temperature was 40°C and the reaction time was 1h. The mixed solution was then centrifuged to obtain a supernatant after acid leaching and a graphite slurry to be modified. The graphite slurry to be modified was washed and dried to obtain 28.71g of graphite to be modified.

[0052] S3: Add 6 wt% sucrose to the graphite to be modified after acid leaching, and then ball mill to obtain a mixed slurry. Then, blow dry the mixture at 150°C for 3 h. Place the obtained modified graphite precursor in a crucible under N 2 The calcination was carried out under atmosphere with a heating rate of 5°C / min to 850°C and kept for 4h to obtain modified graphite.

[0053] S4: Remove other metal impurities from the supernatant after acid leaching in S2 and add NH 4 OH adjusts the pH to between 7 and 8, then introduces carbon dioxide into the solution, and repeats the lithium extraction operation to obtain battery-grade Li 2 CO 3 The mass is 1.47 g. The obtained battery-grade Li 2 CO 3 The total mass is (2.73+1.47)g.

[0054] Comparative Example 3 The difference from Example 3 is that no charging is performed.

[0055] S1: Battery disassembly and electrode crushing. Disassemble the retired lithium battery module into single cells, transfer the single cells to the dew point room for disassembly, take out the lithium-embedded negative electrode, transfer the negative electrode to the crusher and crush it. The crushed negative electrode weighs 15kg.

[0056] S2: Oxidation of graphite carbon and lithium. The crushed negative electrode sheet is transferred to the first reactor via a conveyor belt. The reactor has a volume of 40L. High-purity argon (≥99.9%) is introduced into the reactor in advance to expel the air. Then high-purity oxygen (≥99.9%) is introduced, and the temperature in the reactor rises to 800°C and maintained. The reaction is stopped after continuous introduction of high-purity oxygen for 2 hours. The solids separated from the bottom of the reactor include the copper current collector and some unreacted solids, weighing 4.5kg.

[0057] S3: Pass high-pressure water mist. After the temperature drops to room temperature, continue to spray high-pressure water mist (deionized water, pressure of high-pressure water mist P ≥ 1MPa, cumulative distribution of droplets Dv0.99 < 1000μm on a plane 1m away from the nozzle) into the reactor. Stop after the water in the reactor completely immerses the solids. After 1 hour, pass the solids at the bottom of the reactor through a filter with a pore size of 0.2μm. The weight of the obtained lithium carbonate initial product is 0.4kg. Since the reaction will generate a lot of heat, in order to prevent the lithium carbonate from sticking to the wall and causing low yield and purity, it is necessary to cool the solution by circulating cooling water to keep the temperature below 30°C.

[0058] S4: Washing, centrifugation and drying to obtain high-purity lithium carbonate product. The solid obtained in S3 is washed with pure water solution for 1 hour at 80°C, and the mass of pure water added is 30kg. The washed lithium carbonate is centrifuged and then dried at 120°C to finally obtain 0.3kg of high-purity lithium carbonate product.

[0059] Comparative Example 4 The difference from Example 3 is that high-pressure water mist is not used, but water is directly introduced instead.

[0060] S1: Battery disassembly and electrode crushing. Disassemble the retired lithium battery module into single cells, charge each single cell separately, and charge to the acceptable voltage upper limit (full charge state) according to the attenuation of different single cells. In this embodiment, the lithium iron phosphate single cell is charged at a constant current to 3.65V before charging. After the single cell is fully charged, it is transferred to the dew point room for disassembly, and the negative electrode plate in the lithium embedded state is taken out. The negative electrode plate is transferred to the crusher for crushing. The weight of the crushed negative electrode plate is 15kg.

[0061] S2: Oxidation of graphite carbon and lithium. The crushed negative electrode sheet is transferred to the first reactor via a conveyor belt. The reactor has a volume of 40L. High-purity argon (≥99.9%) is introduced into the reactor in advance to expel the air. Then high-purity oxygen (≥99.9%) is introduced, and the temperature in the reactor rises to 800°C and maintained. The reaction is stopped after continuous introduction of high-purity oxygen for 2 hours. The solids at the bottom of the reactor are separated, including the copper current collector and some unreacted solids, weighing 5kg.

[0062] S3: After the temperature drops to room temperature, deionized water is injected into the bottom of the reactor. The reaction is stopped after the water in the reactor completely submerges the solids. The solids at the bottom of the reactor are filtered through a filter with a pore size of 0.2 μm. The weight of the obtained lithium carbonate initial product is 4.0 kg. Since the reaction generates a lot of heat, in order to prevent the lithium carbonate from sticking to the wall and causing low yield and purity, it is necessary to cool the solution by circulating cooling water to keep the solution temperature below 30°C.

[0063] S4: Washing, centrifugation and drying to obtain high-purity lithium carbonate product. The solid obtained in S3 is washed with pure water solution for 1 hour at 80°C, and the mass of pure water added is 30kg. The washed lithium carbonate is centrifuged and then dried at 120°C to finally obtain 3.7kg of high-purity lithium carbonate product.

[0064] Table 1 As shown in Table 1, the present invention charges the retired lithium-ion battery and fully transfers the remaining reversible lithium source to the negative electrode graphite layer, which is conducive to the efficient extraction of lithium, and the yield is greatly improved. Then, carbon dioxide is generated by high-temperature oxidation of graphite carbon, and carbon dioxide does not need to be introduced from the outside. When graphite is oxidized at high temperature, the lithium embedded in the graphite layered structure can also react fully, and the solubility of carbon dioxide in water is improved by high-pressure water mist. The separation and purification of lithium sources can be maximized by this method. Example 1-3 is compared with Comparative Example 1-2, which shows that the present invention has a higher lithium extraction rate than the prior art method, and can more efficiently and conveniently achieve the separation and purification of lithium sources. Comparative Example 3 shows that by charging the retired lithium-ion battery, the remaining reversible lithium source is fully transferred to the negative electrode graphite layer, which can significantly improve the yield of lithium carbonate. Comparative Example 4 shows that high-pressure water mist can significantly improve the solubility of carbon dioxide in water, and the water mist can fully contact the carbon dioxide generated by graphite oxidation, increase the reaction rate, and improve efficiency.

[0065] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for recovering and extracting lithium from retired lithium-ion batteries. It is characterized in that The steps include: S1: After the retired lithium-ion battery is fully charged, the negative electrode sheet is removed and crushed. This process is carried out in a glove box or dew point room; S2: The crushed negative electrode sheet is transferred to a reactor protected by an inert atmosphere, and then high-purity oxygen is introduced and the temperature is increased for reaction; S3: After the reaction is completed, the temperature is lowered to room temperature and high-pressure water mist is introduced; S4: The solid obtained in S3 is sieved, washed, centrifuged and dried to obtain a lithium carbonate product.

2. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, It is characterized in that The high-purity oxygen described in S2 has a purity of ≥99.9%.

3. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, It is characterized in that The heating temperature in S2 is 500-1500°C, and the reaction time is 30 min-5 h.

4. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, It is characterized in that The pressure of the high-pressure water mist described in S3 is P ≥ 1 MPa, and the cumulative distribution of droplets on the plane 1 m away from the nozzle is Dv0.99 < 1000 μm.

5. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, It is characterized in that The high-pressure water mist injection time described in S3 is 20 minutes to 3 hours.

6. The method for recovering and extracting lithium from retired lithium-ion batteries according to any one of claims 1 to 5, It is characterized in that The negative electrode sheet in S1 uses graphite as the negative electrode active material; the dew point relative humidity in the dew point room is controlled to be ≤-50°C; the oxygen content in the glove box is ≤1 ppm, and the water content is ≤1 ppm.

7. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, It is characterized in that The sieve used for sieving in S4 has a pore size of ≤0.5 μm.

8. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, It is characterized in that The washing in S4 is performed by water washing, and the mass ratio of pure water added to the precipitate is ≥5:

1.

9. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, 7 or 8, It is characterized in that The centrifugation speed in S4 is not less than 1000 rpm.

10. The method for recovering and extracting lithium from retired lithium-ion batteries according to claim 1, 7 or 8, It is characterized in that The drying temperature in S4 is not less than 100°C.

Citation Information

Cited By

  • Carbon-coated lithium iron phosphate material, preparation method and application thereof

    CN120453359A