Component design method suitable for nickel-based single crystal superalloy thin-wall mold filling, nickel-based single crystal superalloy and preparation method and application of nickel-based single crystal superalloy

By regulating the chemical composition and process of nickel-based single-crystal high-temperature alloy, the problem of incomplete filling of nickel-based single-crystal high-temperature alloy thin-walled structural parts during casting is solved, and the thin-walled filling capability of nickel-based single-crystal high-temperature alloy is realized. Improved, suitable for the needs of high-temperature pre-turbocharged aircraft engines.

CN118979176APending Publication Date: 2024-11-19BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411071167.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The thin-walled structural parts of nickel-based single crystal high-temperature alloy are prone to casting defects with incomplete filling during casting, which leads to severe challenges in precision casting of thin-walled structural parts, especially in the high pre-turbine temperature requirements of turbine blades in aircraft engines. In the case of increasing, the prior art will find it difficult to effectively solve this problem.

Method used

By combining the physical properties of Scheil-Gulliver and the liquid-solid phase, Jmatpro software was used to analyze the influence of alloy elements on surface tension and liquid viscosity, and regulate the chemical composition of nickel-based single-crystalline high-temperature alloys, including the appropriate addition of Al, Mo, Cr, and Co. To reduce surface tension and liquid viscosity and reduce the addition of refractory elements, a nickel-based single-crystalline high-temperature alloy with good filling ability is prepared by using directed solidification, solid solution treatment and aging treatment processes.

Benefits of technology

The thin-wall filling capacity of nickel-based single crystal high-temperature alloy is improved, ensuring the filling integrity of casting, suitable for the needs of high pre-turbine temperature in aircraft engines, and improving the performance of turbine blades.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979176A_ABST
    Figure CN118979176A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of alloy materials, and particularly relates to a composition design method suitable for thin-wall mold filling of nickel-based single-crystal superalloy, the nickel-based single-crystal superalloy and a preparation method and application of the nickel-based single-crystal superalloy. The nickel-based single-crystal high-temperature alloy provided by the invention comprises the following chemical components in percentage by mass: 7-9% of Al, 9-12% of Mo, 1-3% of Re, 2.5-4% of Ta, 1-1.5% of Cr, 0.005-0.02% of C and the balance of Ni. The nickel-based single-crystal high-temperature alloy has good mold filling capacity under the combined action of all elements with specific dosage, and is suitable for thin-wall mold filling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of alloy materials, and in particular relates to a composition design method suitable for nickel-based single crystal high-temperature alloy thin-wall filling, a nickel-based single crystal high-temperature alloy, and a preparation method and application thereof. Background Art

[0002] Nickel-based single crystal high-temperature alloys have become the most commonly used turbine blade material for aircraft engines due to their excellent comprehensive mechanical properties. With the development of science and technology, higher performance requirements are placed on aircraft engines, such as wide bypass ratio, wide compression ratio and high turbine inlet temperature. Among them, high turbine inlet temperature is an important indicator for evaluating aircraft engine performance. With the increase in the thrust-to-weight ratio of aircraft engines, the demand for turbine inlet temperature has now increased to 2400K. At present, the main ways to increase the turbine inlet temperature include coating thermal barrier coatings and adopting high-efficiency air cooling technology. The development of high-efficiency air cooling technology has gone through technical development stages such as single-channel film cooling, composite cooling, and double-wall super air cooling.

[0003] In recent years, the double-wall super-air cooling technology has greatly increased the temperature before the turbine. The double-wall structure makes the single-crystal turbine blade a hollow thin-wall structure with two layers inside and outside. The thinnest part of the blade can reach 0.4-0.5mm. The thin-wall design of the turbine blade leads to the casting defect of incomplete filling of the thin wall of the blade with a specified height. The above problems have posed severe challenges to the precision casting of thin-walled structural parts.

[0004] Therefore, for thin-wall structures, designing a single crystal high-temperature alloy suitable for thin-wall filling has important theoretical guiding significance and practical value for the development of double-wall blades and the research and development of a new generation of aircraft engines. Summary of the invention

[0005] In view of this, the present invention provides a composition design method suitable for thin-wall filling of nickel-based single crystal high-temperature alloys, a nickel-based single crystal high-temperature alloy and a preparation method and application thereof. The nickel-based single crystal high-temperature alloy provided by the present invention has good filling ability and can be suitable for thin-wall filling.

[0006] In order to solve the above technical problems, the present invention provides a composition design method suitable for nickel-based single crystal high-temperature alloy thin-wall filling, comprising the following steps:

[0007] Step 1: Combining the physical properties of Scheil-Gulliver and liquid-solid phases, using Jmatpro software to obtain the effect of any alloy element on the surface tension of the alloy liquid, the alloy element being an element contained in the nickel-based single crystal high-temperature alloy;

[0008] Step 2: Combine Scheil-Gulliver and the physical properties of liquid and solid phases, and use Jmatpro software to obtain the effect of alloy elements on the viscosity of alloy liquid;

[0009] Step 3: Combining Scheil-Gulliver and the physical properties of liquid and solid phases, the Jmatpro software is used to obtain the effect of the addition amount of C element on the surface tension and viscosity of the alloy liquid; there is no time sequence restriction between steps 1, 2, and 3;

[0010] Step 4: Refer to the analysis results of steps 1 to 3 to adjust the chemical composition of the nickel-based single crystal high-temperature alloy.

[0011] The present invention provides a nickel-based single crystal high-temperature alloy, comprising the following chemical components in percentage by mass:

[0012]

[0013] Preferably, the chemical components include the following mass percentages:

[0014]

[0015] The present invention also provides a method for preparing the nickel-based single crystal high-temperature alloy described in the above technical solution, comprising the following steps:

[0016] Mixing the raw materials according to the element ratio and smelting them to obtain a melt;

[0017] placing the melt in a mold for directional solidification to obtain a green body;

[0018] The blank is subjected to solution treatment and aging treatment in sequence to obtain the nickel-based single crystal high-temperature alloy.

[0019] Preferably, the smelting temperature is 1500-1700° C., and the smelting holding time is 1-4 hours.

[0020] Preferably, the pulling rate of the directional solidification is 1 to 5 mm / min, and the temperature gradient is 20 to 40 K / cm.

[0021] Preferably, the solution treatment includes a first solution treatment and a second solution treatment performed sequentially;

[0022] The temperature of the first solution treatment is 1270-1290° C., and the holding time of the first solution treatment is 8-12 hours;

[0023] The temperature of the second solid solution treatment is greater than 1290° C. and less than or equal to 1310° C., and the holding time of the second solid solution treatment is 10 to 15 hours.

[0024] Preferably, the aging treatment includes a first aging treatment and a second aging treatment performed sequentially;

[0025] The temperature of the first aging treatment is 100-300° C. higher than the temperature of the second aging treatment.

[0026] Preferably, the temperature of the first aging treatment is 1000-1100° C., and the holding time of the first aging treatment is 5-10 hours;

[0027] The temperature of the second aging treatment is 800-900° C., and the holding time of the second aging treatment is 40-60 hours.

[0028] The present invention also provides the use of the nickel-based single crystal high-temperature alloy described in the above technical solution or the nickel-based single crystal high-temperature alloy prepared by the preparation method described in the above technical solution in aircraft engines.

[0029] The present invention provides a nickel-based single crystal high temperature alloy, comprising the following chemical components in mass percentage: 7-9% Al, 9-12% Mo, 1-3% Re, 2.5-4% Ta, 1-1.5% Cr, 0.005-0.02% C and the balance Ni. In the present invention, the Al element positively promotes thin-wall filling, the Mo element positively promotes thin-wall filling, the W element has both positive promotion and reverse inhibition effects on thin-wall filling, the Cr element has both positive promotion and reverse inhibition effects on thin-wall filling, the Co element has both positive promotion and reverse inhibition effects on thin-wall filling, the C element promotes thin-wall filling when added in an appropriate amount, and causes a violent shell reaction when added in an excessive amount, the Re element reversely inhibits thin-wall filling, and the Ta element reversely inhibits thin-wall filling. The present invention improves the anti-oxidation and anti-corrosion properties of the alloy by adding an appropriate amount of Cr element, and adds an appropriate amount of C element to promote thin-wall filling. At the same time, Mo, an element that promotes thin-wall filling, is used as much as possible to replace refractory elements (Re, Cr, W and Co), and reduce the addition of other refractory elements. Ta, W, Re have a strong positive correlation with surface tension, while Al, Cr, Co, etc. have a strong negative correlation with surface tension. Ta, Re, Cr, Co have a strong positive correlation with the viscosity of the alloy liquid, while W and Mo have a weak positive correlation with the viscosity of the alloy liquid, and the Al element has a negative correlation with the viscosity of the alloy liquid. The addition of trace element C can significantly reduce the surface tension and viscosity of the alloy liquid. Under the joint action of specific amounts of various elements, the present invention enables the nickel-based single crystal high-temperature alloy to have good filling ability, is suitable for thin-wall filling, and can achieve complete filling casting. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the forces during the alloy liquid filling process;

[0031] Figure 2 This is the result diagram of the influence of alloy elements Al, Ta, Mo, Re, Cr, W, and Co on surface tension;

[0032] Figure 3This is the result diagram of the influence of alloy elements Al, Ta, Mo, Re, Cr, W, and Co on the viscosity of alloy liquid;

[0033] Figure 4 It is a dot-line diagram showing the effect of the amount of C element added on the surface tension;

[0034] Figure 5 It is a dot-line diagram showing the effect of the addition amount of C element on the viscosity of the alloy liquid;

[0035] Figure 6 is the thickness of the shell reaction layer of the alloys prepared in Example 1 and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0036] The present invention provides a composition design method suitable for nickel-based single crystal high-temperature alloy thin-wall filling, comprising the following steps:

[0037] Step 1: Combining the physical properties of Scheil-Gulliver and liquid-solid phases, using Jmatpro software to obtain the effect of any alloy element on the surface tension of the alloy liquid, the alloy element being an element contained in the nickel-based single crystal high-temperature alloy;

[0038] Step 2: Combine Scheil-Gulliver and the physical properties of liquid and solid phases, and use Jmatpro software to obtain the effect of alloy elements on the viscosity of alloy liquid;

[0039] Step 3: Combining Scheil-Gulliver and the physical properties of liquid and solid phases, the Jmatpro software is used to obtain the effect of the addition amount of C element on the surface tension and viscosity of the alloy liquid; there is no time sequence restriction between steps 1, 2, and 3;

[0040] Step 4: Refer to the analysis results of steps 1 to 3 to adjust the chemical composition of the nickel-based single crystal high-temperature alloy.

[0041] In the present invention, Figure 1 Figure 1 is a schematic diagram of the forces acting on the alloy liquid during the filling process. The driving force of the alloy liquid filling process is calculated by formula 1:

[0042] P=ΔP-P L Formula (1);

[0043] Where ΔP is the driving force generated by the liquid pouring system, P L is the resistance of alloy liquid filling, and P is the driving force of alloy liquid filling.

[0044] The alloy liquid filling resistance is calculated according to formula (2):

[0045] P L =4σ / b Formula (2);

[0046] Among them, σ is the surface tension and b is the thickness of the thin-walled alloy liquid.

[0047] It can be seen from formula (1) and formula (2) that the alloy liquid filling resistance is caused by the surface tension of the alloy liquid. Low surface tension is conducive to reducing the alloy liquid filling resistance and promoting the filling process of thin-walled parts.

[0048] Based on the idea of ​​combining Scheil-Gulliver's calculation with the physical properties of liquid and solid phases, the present invention uses Jmatpro software to batch calculate the effects of typical alloying elements Al, Ta, Mo, Re, Cr, W, and Co on the surface tension of alloy liquid. The results are as follows: Figure 2 In the present invention, the results are qualitative results. Figure 2 It can be seen that above 1500°C, Ta, W, and Re have a strong positive correlation with surface tension, while Al, Cr, and Co have a strong negative correlation with surface tension.

[0049] In the present invention, the alloy liquid flow rate between the thin walls is positively correlated with the alloy filling capacity, and the value of the alloy liquid flow rate between the thin walls is calculated by formula (3):

[0050]

[0051] Wherein, W is the width of thin-wall alloy liquid, b is the thickness of thin-wall alloy liquid, η is the viscosity of alloy liquid, and Q is the alloy liquid flow rate between thin walls.

[0052] It can be seen from formula (3) that low alloy liquid viscosity is conducive to increasing the alloy liquid flow rate between thin walls and promoting the filling process of thin-walled parts.

[0053] Based on the idea of ​​combining Scheil-Gulliver calculation with the physical properties of liquid and solid phases, the present invention uses Jmatpro software to batch calculate the effects of typical alloying elements such as Al, Ta, Mo, Re, Cr, W, Co, etc. on the viscosity of alloy liquid. The results are as follows: Figure 3 As shown in the figure, the larger the value, the stronger the positive correlation between the element content and the viscosity of the alloy liquid. In the present invention, the result is a qualitative result. Figure 3 It can be seen that above 1500℃, Ta, Re, Cr, Co have a strong positive correlation with the viscosity of the alloy liquid, W, Mo have a weak positive correlation with the viscosity of the alloy liquid, and the Al element has a negative correlation with the viscosity of the alloy liquid.

[0054] Trace element C is a key element in nickel-based single crystal high-temperature alloys. Based on the idea of ​​combining Scheil-Gulliver's calculation with the physical properties of liquid and solid phases, the present invention uses Jmatpro software to batch calculate the effect of adding C element on surface tension and alloy liquid viscosity. The results are as follows Figure 4 and Figure 5 As shown, Figure 4 This is a dot-line diagram showing the effect of adding C element on surface tension. Figure 5 This is a dot-line diagram showing the effect of the addition of C element on the viscosity of the alloy liquid. Figure 4 and Figure 5 It can be seen that above 1500℃, the addition of trace element C can significantly reduce the surface tension and viscosity of the alloy liquid.

[0055] In the present invention, refractory elements such as W, Cr, Mo, Re, and Ru will significantly increase element segregation, and excessive addition of trace element C will significantly cause formwork reaction.

[0056] Based on the above analysis results, the present invention proposes an alloy composition design concept suitable for nickel-based single crystal high-temperature alloy thin-wall filling:

[0057] (1) To reduce the surface tension of the alloy liquid and promote the thin-wall filling process of the nickel-based single crystal high-temperature alloy, the content of Al, Cr, and Co should be increased, and the content of Ta, W, and Re should be reduced.

[0058] (2) To reduce the viscosity of the alloy liquid and promote the thin-wall filling process of the nickel-based single crystal high-temperature alloy, the content of Al, Mo, and W elements should be increased, and the content of Ta, Re, Cr, and Co elements should be reduced.

[0059] (3) An appropriate amount of trace element C should be added to promote the thin-wall filling process of nickel-based single crystal high-temperature alloys, but it should be noted that excessive addition should be avoided to avoid violent mold shell reaction.

[0060] (4) In order to reduce the degree of element segregation after thin-wall filling of nickel-based single crystal high-temperature alloy, the total addition content of refractory elements such as W, Mo, Re, Co, and Cr should be reduced.

[0061] The present invention provides a nickel-based single crystal high-temperature alloy, comprising the following chemical components in percentage by mass:

[0062]

[0063] The present invention analyzes and limits the element composition of the alloy according to the composition design method of the nickel-based single crystal high-temperature alloy, and obtains a nickel-based single crystal high-temperature alloy with good filling ability.

[0064] Calculated by mass percentage, the nickel-based single crystal high-temperature alloy provided by the present invention includes 7-9% Al, preferably 7.5-8.5%.

[0065] Calculated by mass percentage, the nickel-based single crystal high-temperature alloy provided by the present invention comprises 9-12% Mo, preferably 10-11%.

[0066] Calculated by mass percentage, the nickel-based single crystal high-temperature alloy provided by the present invention includes 1-3% Re, preferably 1.5-2.5%.

[0067] Calculated by mass percentage, the nickel-based single crystal high-temperature alloy provided by the present invention includes 2.5-4% Ta, preferably 3-3.5%.

[0068] Calculated by mass percentage, the nickel-based single crystal high-temperature alloy provided by the present invention includes 1 to 1.5% Cr, preferably 1.2 to 1.4%.

[0069] Calculated by mass percentage, the nickel-based single crystal high-temperature alloy provided by the present invention includes 0.005-0.02% C, preferably 0.01-0.015%.

[0070] Measured in percentage by mass, the nickel-based single crystal high-temperature alloy provided by the present invention includes a balance of Ni.

[0071] The present invention also provides a method for preparing the nickel-based single crystal high-temperature alloy described in the above technical solution, comprising the following steps:

[0072] Mixing the raw materials according to the element ratio and smelting them to obtain a melt;

[0073] placing the melt in a mold for directional solidification to obtain a green body;

[0074] The blank is subjected to solution treatment and aging treatment in sequence to obtain the nickel-based single crystal high-temperature alloy.

[0075] The present invention mixes the raw materials according to the element ratio and smelts them to obtain a melt. The present invention has no special requirements on the source and type of the raw materials, and conventional materials in the field can be used. In an embodiment of the present invention, the purity of the raw materials is preferably 99.99% or more. In the present invention, the smelting temperature is preferably 1500-1700°C, more preferably 1550-1650°C; the smelting holding time is preferably 1-4h, more preferably 2-3h.

[0076] After obtaining the melt, the present invention places the melt in a mold for directional solidification to obtain a blank. In the present invention, the material of the mold is preferably alumina. The present invention has no special requirements for the mold, and it can be designed according to the required shape and size of the alloy. In the present invention, the directional solidification method is preferably Bridgman directional solidification; the pulling rate of the directional solidification is preferably 1 to 5 mm / min, more preferably 2 to 4 mm / min; the temperature gradient of the directional solidification is preferably 20 to 40 K / cm, more preferably 25 to 35 K / cm. The present invention adopts the Bridgman directional solidification method for directional solidification to ensure that a single crystal alloy is obtained.

[0077] After obtaining the blank, the present invention sequentially performs a solution treatment and an aging treatment on the blank to obtain the nickel-based single crystal high-temperature alloy. In the present invention, the solution treatment includes a first solution treatment and a second solution treatment performed sequentially. In the present invention, the temperature of the first solution treatment is preferably 1270-1290°C, more preferably 1275-1285°C; the holding time of the first solution treatment is preferably 8-12h, more preferably 9-11h. In the present invention, the temperature of the second solution treatment is preferably greater than 1290 and less than or equal to 1310°C, more preferably 1295-1305°C; the holding time of the second solution treatment is preferably 10-15h, more preferably 11-13h.

[0078] In the present invention, the aging treatment preferably includes a first aging treatment and a second aging treatment performed sequentially. In the present invention, the temperature of the first aging treatment is preferably 1000-1100°C, more preferably 1050-1080°C; the holding time of the first aging treatment is preferably 5-10h, more preferably 6-8h. In the present invention, the temperature of the second aging treatment is preferably 800-900°C, more preferably 850-880°C; the holding time of the second aging treatment is preferably 40-60h, more preferably 45-55h. In the present invention, the temperature of the first aging treatment is preferably 100-300°C higher than the temperature of the second aging treatment, more preferably 150-250°C higher.

[0079] The present invention also provides the use of the nickel-based single crystal high-temperature alloy described in the above technical solution or the nickel-based single crystal high-temperature alloy prepared by the preparation method described in the above technical solution in aircraft engines.

[0080] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0081] Example 1

[0082] 211 g of high-purity 99.99% aluminum source, 271 g of high-purity 99.99% molybdenum source, 31 g of high-purity 99.99% rhenium source, 76 g of high-purity 99.99% tantalum source, 31 g of high-purity 99.99% chromium source, 0.16 g of high-purity 99.99% carbon source, and 2380 g of high-purity 99.99% nickel source were mixed and smelted at 1600° C. for 3 hours to obtain a melt;

[0083] The molten metal is placed in an alumina mold shell and directionally solidified at a pulling rate of 3 mm / min and a temperature gradient of 25 K / cm according to the Bridgman directional solidification method to obtain a green body;

[0084] The blank is subjected to a first solid solution treatment at 1280°C for 10 hours and then to a second solid solution treatment at 1300°C for 12 hours; after the solid solution treatment, the product is subjected to a first aging treatment at 1070°C for 8 hours and then to a second aging treatment at 880°C for 50 hours to obtain a nickel-based single crystal high-temperature alloy; the chemical composition of the nickel-based single crystal high-temperature alloy is 7% Al, 9% Mo, 1% Re, 2.5% Ta, 1.0% Cr, 0.005% C and the remainder Ni.

[0085] Example 2

[0086] 270 g of high-purity 99.99% aluminum source, 360 g of high-purity 99.99% molybdenum source, 90 g of high-purity 99.99% rhenium source, 120 g of high-purity 99.99% tantalum source, 45 g of high-purity 99.99% chromium source, 0.3 g of high-purity 99.99% carbon source, and 2115 g of high-purity 99.99% nickel source were mixed and smelted at 1600° C. for 3 hours to obtain a melt;

[0087] The molten metal is placed in an alumina mold shell and solidified according to the Bridgman directional solidification method at a pulling rate of 3 mm / min and a temperature gradient of 30 K / cm to obtain a green body;

[0088] The blank is subjected to a first solid solution treatment at 1290°C for 10 hours and then to a second solid solution treatment at 1310°C for 12 hours; after the solid solution treatment, the product is subjected to a first aging treatment at 1100°C for 8 hours and then to a second aging treatment at 900°C for 50 hours to obtain a nickel-based single crystal high-temperature alloy; the chemical composition of the nickel-based single crystal high-temperature alloy is 9% Al, 12% Mo, 3% Re, 4% Ta, 1.5% Cr, 0.01% C and the remainder Ni.

[0089] Comparative Example 1

[0090] 186g of high-purity 99.99% aluminum source, 45g of high-purity 99.99% molybdenum source, 90g of high-purity 99.99% rhenium source, 189g of high-purity 99.99% tantalum source, 210g of high-purity 99.99% chromium source, 1.5g of high-purity 99.99% carbon source, 225g of high-purity 99.99% cobalt source, 150g of high-purity 99.99% tungsten source, and 1904g of high-purity 99.99% nickel source were mixed and smelted at 1600°C for 3h to obtain a melt;

[0091] The molten metal is placed in an alumina mold shell and solidified according to the Bridgman directional solidification method at a pulling rate of 3 mm / min and a temperature gradient of 30 K / cm to obtain a green body;

[0092] The blank is subjected to a first solid solution treatment at 1260°C for 8 hours and then to a second solid solution treatment at 1300°C for 4 hours; after the solid solution treatment, the product is subjected to a first aging treatment at 1120°C for 4 hours and then to a second aging treatment at 900°C for 12 hours to obtain a nickel-based single crystal high-temperature alloy; the chemical composition of the nickel-based single crystal high-temperature alloy is 6.2% Al, 1.5% Mo, 3% Re, 6.3% Ta, 7% Cr, 7.5% Co, 5% W, 0.05% C and the remainder Ni.

[0093] Comparative Example 2

[0094] 177g of high-purity 99.99% aluminum source, 36g of high-purity 99.99% molybdenum source, 120g of high-purity 99.99% rhenium source, 117g of high-purity 99.99% tantalum source, 144g of high-purity 99.99% chromium source, 4.5g of high-purity 99.99% carbon source, 273g of high-purity 99.99% cobalt source, 258g of high-purity 99.99% tungsten source, and 1870g of high-purity 99.99% nickel source were mixed and smelted at 1600°C for 3h to obtain a melt;

[0095] The molten metal is placed in an alumina mold shell and solidified according to the Bridgman directional solidification method at a pulling rate of 3 mm / min and a temperature gradient of 30 K / cm to obtain a green body;

[0096] The blank is subjected to a first solid solution treatment at 1200°C for 10 hours and then to a second solid solution treatment at 1280°C for 4 hours; after the solid solution treatment, the product is subjected to a first aging treatment at 1140°C for 4 hours and then to a second aging treatment at 860°C for 24 hours to obtain a nickel-based single crystal high-temperature alloy; the chemical composition of the nickel-based single crystal high-temperature alloy is 5.9% Al, 1.2% Mo, 4% Re, 3.9% Ta, 4.8% Cr, 9.1% Co, 8.6% W, 0.15% C and the remainder Ni.

[0097] Comparative Example 3

[0098] 174 g of high-purity 99.99% aluminum source, 30 g of high-purity 99.99% molybdenum source, 144 g of high-purity 99.99% rhenium source, 243 g of high-purity 99.99% tantalum source, 90 g of high-purity 99.99% chromium source, 1.2 g of high-purity 99.99% carbon source, 360 g of high-purity 99.99% cobalt source, 180 g of high-purity 99.99% tungsten source, and 1778 g of high-purity 99.99% nickel source were mixed and smelted at 1600° C. for 3 hours to obtain a melt;

[0099] The molten metal is placed in an alumina mold shell and solidified according to the Bridgman directional solidification method at a pulling rate of 3 mm / min and a temperature gradient of 30 K / cm to obtain a green body;

[0100] The blank is subjected to a first solid solution treatment at 1315°C for 16 hours and then to a second solid solution treatment at 1345°C for 16 hours; after the solid solution treatment, the product is subjected to a first aging treatment at 1160°C for 4 hours and then to a second aging treatment at 880°C for 24 hours to obtain a nickel-based single crystal high-temperature alloy; the chemical composition of the nickel-based single crystal high-temperature alloy is 5.8% Al, 1% Mo, 4.8% Re, 8.1% Ta, 3% Cr, 12% Co, 6% W, 0.04% C and the remainder Ni.

[0101] The alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 3 were used to fill the mold, and the filling height and filling rate were obtained and are listed in Table 1.

[0102] Table 1 Filling properties of alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 3

[0103]

[0104] It can be seen from the results in Table 1 that Comparative Example 1 contains relatively high levels of Cr, Co, and Ta elements that are not conducive to filling, and the filling is incomplete, with a filling rate of 61%; Comparative Example 2 contains relatively high levels of refractory elements such as Re, Co, and W that are not conducive to filling, resulting in severe dendrite segregation, and the alloy contains an extremely high C content, which promotes the thin-wall filling process, but at the same time causes severe mold shell reaction, with a filling rate of 75%; Comparative Example 3 contains relatively high levels of Ta elements and refractory elements such as Re, Co, and W that are not conducive to filling, with a filling rate of 57%, and causes severe dendrite segregation.

[0105] The nickel-based single crystal high-temperature alloy designed according to the design method provided by the present invention has good mold filling ability, and the mold filling rate is 84-86%.

[0106] The EDS energy spectrum method was used to quantitatively analyze the element segregation behavior of the alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 3 in terms of dendrite trunk ratio and inter-dendrite ratio. The segregation ratio is the ratio of the dendrite trunk element to the inter-dendrite element. The deviation from 1 indicates the degree of element segregation. The results are shown in Table 2.

[0107] Table 2 Element segregation behavior of the embodiments and comparative examples

[0108]

[0109] According to the results in Table 2, when the total amount of refractory elements (Cr, Mo, Re) added in Example 1 is 11%, the element segregation behavior is not obvious; when the total amount of refractory elements (Cr, Mo, Re) added in Example 2 is 16.5%, the element segregation behavior increases, but is not obvious; when the total amount of refractory elements (Re, Cr, Mo, W and Co) added in Comparative Example 1 is 24%, the Re element produces obvious element segregation; when the total amount of refractory elements (Re, Cr, Mo, W and Co) added in Comparative Example 2 is 27.7%, Re, Ta, W and other elements produce very obvious element segregation; when the total amount of refractory elements (Re, Cr, Mo, W and Co) added in Comparative Example 3 is 26.8%, Re, Ta, W and other elements produce very obvious element segregation; the element segregation behavior of the thin-walled part after solidification is positively correlated with the total amount of refractory elements such as Re, Co, W and other elements added in the alloy liquid, and the total amount of refractory elements added should be controlled.

[0110] The thickness of the shell reaction layer of the alloys prepared in Examples 1 to 2 and Comparative Examples 1 to 3 was collected by field emission scanning electron microscopy. The thickness of the shell reaction layer is shown in Table 3. The collected photos are shown in Table 3. Figure 6 As shown, Figure 6 It is a side scan image of the alloys prepared in Example 1 and Comparative Examples 1 to 3.

[0111] Table 3 Element segregation behavior of examples and comparative examples

[0112] Example Thickness of shell reaction layer Example 1 3.2μm Example 2 3.9μm Comparative Example 1 4.9μm Comparative Example 2 81.2μm Comparative Example 3 4.55μm

[0113] Combining Table 3 and Figure 6 It can be seen that Comparative Example 2 produces a very serious shell reaction due to its higher C content.

[0114] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A composition design method suitable for thin-wall filling of nickel-based single crystal high-temperature alloys, characterized in that: The following steps are involved: Step 1: Combining the physical properties of Scheil-Gulliver and liquid-solid phases, using Jmatpro software to obtain the effect of any alloy element on the surface tension of the alloy liquid, the alloy element being an element contained in the nickel-based single crystal high-temperature alloy; Step 2: Combine Scheil-Gulliver and the physical properties of liquid and solid phases, and use Jmatpro software to obtain the effect of alloy elements on the viscosity of alloy liquid; Step 3: Combining Scheil-Gulliver and the physical properties of liquid and solid phases, the Jmatpro software is used to obtain the effect of the addition amount of C element on the surface tension and viscosity of the alloy liquid; there is no time sequence restriction between steps 1, 2, and 3; Step 4: Refer to the analysis results of steps 1 to 3 to adjust the chemical composition of the nickel-based single crystal high-temperature alloy.

2. A nickel-based single crystal high temperature alloy, characterized in that: Includes the following chemical components in percentage by mass:

3. The nickel-based single crystal high temperature alloy according to claim 2, characterized in that: Includes the following chemical components in percentage by mass:

4. The method for preparing the nickel-based single crystal high-temperature alloy according to claim 2 or 3, comprising the following steps: Mixing the raw materials according to the element ratio and smelting them to obtain a melt; placing the melt in a mold for directional solidification to obtain a green body; The blank is subjected to solution treatment and aging treatment in sequence to obtain the nickel-based single crystal high-temperature alloy.

5. The preparation method according to claim 4, characterized in that: The smelting temperature is 1500-1700° C., and the smelting insulation time is 1-4 hours.

6. The preparation method according to claim 4, characterized in that: The pulling rate of the directional solidification is 1-5 mm / min, and the temperature gradient is 20-40 K / cm.

7. The preparation method according to claim 4, characterized in that: The solution treatment includes a first solution treatment and a second solution treatment performed sequentially; The temperature of the first solution treatment is 1270-1290° C., and the holding time of the first solution treatment is 8-12 hours; The temperature of the second solid solution treatment is greater than 1290° C. and less than or equal to 1310° C., and the holding time of the second solid solution treatment is 10 to 15 hours.

8. The preparation method according to claim 4, characterized in that: The aging treatment includes a first aging treatment and a second aging treatment performed sequentially; The temperature of the first aging treatment is 100-300° C. higher than the temperature of the second aging treatment.

9. The preparation method according to claim 8, characterized in that: The temperature of the first aging treatment is 1000-1100° C., and the holding time of the first aging treatment is 5-10 hours; The temperature of the second aging treatment is 800-900° C., and the holding time of the second aging treatment is 40-60 hours.

10. Use of the nickel-based single crystal high-temperature alloy according to claim 2 or 3 or the nickel-based single crystal high-temperature alloy prepared by the preparation method according to any one of claims 4 to 9 in aircraft engines.