High-conductivity ultrahigh-strength aluminum alloy single wire and production process thereof
By optimizing the grain structure and aging process in aluminum alloy wires, combining the synergistic effects of multiple elements, the problem of both conductivity improvement and strength is solved, the balance between high conductivity and high strength is achieved, and the aluminum alloy wire is improved. mechanical properties and thermal stability.
Patent Information
- Application Number
- CN202411061952.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
It is difficult for existing aluminum alloy wires to take into account both strength and elongation while improving the conductivity, resulting in an increase in conductivity that will lead to a decrease in strength and elongation, making it difficult to balance the two.
By adding multiple elements on the basis of the Mg2Si phase, synergistic improvement of alloy performance, optimizing the grain structure, using the solid solution and aging process intervention of the Al3Fe and Mg2Si phases, yttrium elements are added to form a dense oxide film, and the three-stage aging process is adopted and The phased aging process controls crystal precipitation and grain boundary distribution to ensure that the alloy maintains excellent performance after thermal cycling.
The balance of high conductivity and high strength is achieved, the comprehensive mechanical properties and thermal stability of the alloy are improved, the crystal phase dislocation and corrosion are prevented, and the internal structural density and external surface stability of the aluminum alloy wire are enhanced.
Smart Images

Figure CN118979179A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-conductivity ultra-high-strength aluminum alloy single wire and a production process thereof, belonging to the technical field of preparation of overhead conductors for overhead power transmission lines. Background Art
[0002] In the field of modern overhead power transmission, the toughness and weather resistance of aluminum alloy wires are key factors in ensuring power transmission. Due to its high strength, light weight, good conductivity and corrosion resistance, it can effectively reduce energy loss during power transmission and increase the reliability of the power transmission process. With the continuous advancement of technology and the growing demand of the power industry, the performance improvement of aluminum alloy conductors is particularly critical at the technical level. Good aluminum alloy single wires mean moving towards a more efficient and reliable power system, which is of great significance to supporting the upgrade of future energy facilities. The current aluminum alloy wires mainly include smelting, refining and purification, online impurity removal, continuous casting, online solid solution, continuous casting and rolling, wire drawing deformation and artificial aging treatment. Its process mainly focuses on improving the microcrystalline performance of metals and optimizing existing processes, but it has not achieved a fundamental breakthrough. There is a balance between the strength and conductivity of aluminum alloy wires. Improving its conductivity may lead to a decrease in its strength and elongation. How to improve the conductivity of aluminum alloy wires while taking into account its strength has become a technical problem that is difficult to solve in the current industry. Summary of the invention
[0003] The object of the present invention is to provide a high-conductivity ultra-high-strength aluminum alloy single wire.
[0004] The technical solution for achieving the purpose of the present invention is: a high conductivity ultra-high strength aluminum alloy single wire, whose composition is 0.60% to 0.80% silicon, 0.65% to 0.85% magnesium, 0.14% to 0.25% iron, 0.05% to 0.15% scandium, 0.01% to 0.03% copper, 0.01% to 0.15% yttrium, 0.001% to 0.015% titanium, V+Cr≤0.005%, and the rest is aluminum and other inevitable trace impurity elements.
[0005] Based on the Mg2Si phase, the present invention uses multiple elements to synergistically improve the alloy performance. In the range of Mg / Si: = 0.92 to 1.25, the grain structure of the aluminum alloy undergoes a significant transformation process, evolving from a relatively complex form to a highly uniform equiaxed grain structure. This microstructure optimization not only promotes the uniform distribution of grain boundaries, but also greatly enhances the comprehensive mechanical properties of the alloy material. In general, the above alloy uses the high-temperature stable state of Al3Fe to limit the growth range of crystals to prevent them from growing too long, adds titanium during the stirring process to increase the number of non-uniform nucleation points to promote stable crystal precipitation, uses Mg2Si to strengthen the alloy as a whole and prevent crystal phase dislocation, thereby improving crystal regularity, and uses copper to intervene in the solid solution and aging process of Al3Fe and Mg2Si phases to effectively prevent them from melting back, ensuring that the alloy continues to maintain its excellent mechanical properties after undergoing thermal cycles, and adds yttrium before purifying and casting the alloy to promote the formation of a dense oxide film on its surface, thereby resisting high-temperature oxidation and enhancing its internal thermal stability, thereby preventing crystal phase destruction caused by environmental exposure during subsequent processes.
[0006] Furthermore, the present invention also provides a preparation process of a high conductivity ultra-high strength aluminum alloy single wire, which specifically comprises the following steps:
[0007] S1 smelting: smelting aluminum ingots and master alloy ingots according to a predetermined chemical ratio;
[0008] S2 refining: After smelting, the material is transferred to a holding furnace for deep purification to obtain aluminum alloy melt;
[0009] S3 purification and grain optimization: transfer the aluminum alloy melt into the dynamic purification system, and then refine the grains and filter the melt with high precision;
[0010] S4 continuous casting: The alloy liquid after grain optimization is introduced into the casting device, and the aluminum alloy ingot blank is prepared by horizontal continuous casting:
[0011] S5 continuous hot rolling: the aluminum alloy ingot is sent into the temperature control heating system and then evenly heated, and then continuously hot rolled to obtain the alloy rod;
[0012] S6 online quenching: rapid cooling of the alloy rod;
[0013] S7 closes the line tightly;
[0014] S8 Self-aging: The alloy rod after winding is placed at room temperature for self-aging;
[0015] S9 stage aging: the alloy rod after self-aging is placed in the aging furnace for stage aging treatment;
[0016] S10 tensile deformation: the alloy rod that has completed stage aging is subjected to tensile deformation treatment;
[0017] S11 regulatory timeliness.
[0018] Different from the general processing flow, the present application adopts a three-stage aging process, which is self-aging at room temperature after the winding is completed, so that the alloy lattice fracture surface completes the primary healing, and then high-temperature aging treatment is carried out in the aging furnace to further promote the healing of the lattice fracture surface, forming a more stable and denser precipitation phase, and then tensile deformation is carried out on this basis. The probability of alloy phase dislocation is smaller, and its conductivity and strength are higher. In order to heal the alloy section and surface cracks after tensile deformation and repair internal defects, the present application carries out an adjusted aging process after completing the stretching. Its titanium, magnesium, and silicon can form more crystallization nuclei during the aging process, and the crystal regularity is better, and more stable precipitation can be carried out at high temperature. The probability of grain boundary dislocation is smaller, and there are more crystallization nuclei, so the crystal phase is denser, and the yttrium element and the aluminum element work together to form a denser oxide film to prevent alloy corrosion in harsh natural environments, so that the alloy aluminum wire achieves a balance between strength and conductivity.
[0019] Further or optionally, in the S2 refining step, the refining operation range is 720°C to 740°C, the refining time is 30 to 45 minutes, the ratio of refining agent to aluminum alloy solution is 2.5:1000, and then the solution is kept at 730°C to 760°C for 25 minutes.
[0020] Controlling the melting temperature to 720℃~740℃ can effectively prevent the alloy from excessively absorbing hydrogen and reduce the generation of bubbles. It is also beneficial to the full dissolution of alloy elements during the smelting process, effectively removing gases and inclusions, and reducing poor alloy performance. In this operation step, the refining agent is adjusted to 2.5:1000. At this ratio, a balance can be achieved between the refining agent cost and the amount of hydrogen escape, and the gas loss of the finished alloy is smaller.
[0021] Further or optionally, in the S3 purification and grain optimization step, the purification system uses a multi-layer foam ceramic filter plate, the pore size range of the filter plate is 40ppi to 50ppi, the filtration temperature is 740°C, the total amount of the grain optimizer is 0.25%, and the composition is titanium boron rare earth refiner. High-purity nitrogen is used in coordination with the rotor during the purification process.
[0022] During the above operation, a multi-layer foam ceramic filter plate is used, which can not only remove large particles of impurities, but also effectively adsorb and remove fine metal impurities in the aluminum alloy liquid at a deep level, effectively improving the comprehensive performance and purity of the alloy rod; high-purity nitrogen is used to work in conjunction with the rotor, and the rotor and nitrogen can further remove gas impurities in the alloy, further ensuring the high quality of the final product.
[0023] In specific operations, the impurity removal inside the refining furnace is combined with the external online degassing, and a multi-level purification strategy is implemented to achieve a double impurity removal effect. It can effectively remove fine impurities and gaseous pollutants, significantly improve the purity of the aluminum alloy melt, and ensure the purity of the alloy composition before continuous casting.
[0024] Induction heating technology is used in the continuous hot rolling process to achieve uniform heating of the aluminum alloy casting, promote the uniformity of the alloy solid solution during the rolling process, and promote the full precipitation of the alloy phase, so as to improve the overall strength of the alloy and the comprehensive quality of the material.
[0025] Further or optionally, the temperature of the temperature-adjusting heating in the S5 continuous rolling step is 505°C-535°C, the quenching temperature in the S6 online quenching step is 28°C-30°C, the quenching pressure is 500±50kpa, and the quenching process is first immersion water cooling and then air cooling.
[0026] During the specific operation, the rolled alloy rod is first immersed in water quenching and then air-cooled. The temperature difference before and after is as high as 500°C. The alloy rod is cooled rapidly in a short time, and the microstructure of the alloy rod changes rapidly, forming a smaller grain structure. In the process of hardening and precipitation of alloy crystals, it cooperates with the Al3Fe and boron-titanium-based components in the alloy to supply more crystal nuclei and limit the range of crystal growth, thereby effectively inhibiting large-scale phase changes and preventing crystal diffusion, thereby obtaining smaller crystal nuclei than general rapid cooling processes, allowing the alloy to obtain greater strength.
[0027] Further or optionally, the S8 autonomous aging step condition is room temperature, and the aging time is not less than 168 hours; the S9 staged aging condition is 110°C~160°C, and the aging time is 8~24 hours; the step S11 regulatory aging step condition is temperature 120°C~160°C, and the aging time is 5~15 hours.
[0028] The above-mentioned aging process is carried out in three stages, wherein pre-aging is first carried out in a low-temperature stage and then staged aging treatment is carried out, forming a high-density micro-dispersed GP zone inside the alloy, providing abundant nucleation points for subsequent precipitation phases, thus laying the foundation for the structural stability of the alloy; then, final aging treatment is carried out under regulated high-temperature conditions, which not only avoids the solute melting phenomenon, but also significantly improves the distribution uniformity of the precipitate phase.
[0029] Further or optionally, in the S1 smelting step, the alloy ingot used has an aluminum alloy purity of ≥99.70%, a magnetically driven automatic stirring system is used, the furnace temperature is 750-760°C, and the alloy adding components and steps are 10% aluminum-iron intermediate alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additives, 8% aluminum-boron (ALB12) alloy, 10% aluminum-yttrium alloy, 10% aluminum-scandium alloy, and pure magnesium.
[0030] After the alloy raw materials are fed, they are stirred by electromagnetic equipment and kept warm in a holding furnace. At this time, the alloy elements are more evenly dispersed, and the flow and shear force of the electromagnetic stirrer help to refine the grains and promote the β-Fe spheroidization process, thereby reducing the anisotropy of the material.
[0031] The above raw material addition process will affect the crystal phase formation. In this alloy system, the precise addition of scandium (Sc) not only improves the precipitation dynamics of copper (Cu), but also promotes the refinement and uniform distribution of the Cu-Sc eutectic phase in the microstructure. This optimization of the microstructure directly enhances the hardness and strength properties of the alloy; the combined effect of Sc and yttrium (Y) promotes the high-performance Al-Sc-Y phase formation enhancement mechanism; the phase generated by the specific reaction of boron and titanium not only promotes grain refinement, but also helps to capture and remove impurities in the melt, thereby improving the purity of the melt. In terms of the order of addition, iron, silicon and copper alloys have higher melting temperatures, and magnesium alloys have lower melting points but are easily invaded by gases. Therefore, arranging the addition of magnesium alloys after iron, silicon and copper alloys can help reduce gas absorption and related losses in the melt. Preventing boron and titanium-based alloys from being added last can promote grain refinement and improve the purity of the alloy melt. In particular, the addition ratio of scandium (Sc) element has been precisely calibrated and cleverly set in a narrow and efficient range of 0.10wt.% to 0.15wt.%. This adjustment aims to make full use of the scandium element's potential for fine modulation of the aluminum alloy microstructure, and further improve the overall performance of the aluminum alloy by coordinating with the subsequent staged aging treatment process.
[0032] Further or optionally, in the S5 continuous hot rolling step, the hot rolling completion temperature is ≥360°C, in the S6 online quenching step, the cooling temperature is 65°C to 110°C, and in the S7 tight wire winding step, the wire winding temperature is ≤100°C.
[0033] During the rolling process, a billet design with an enhanced cross-sectional size is adopted. The billet has a larger cross-sectional area, which is more conducive to large-scale production in the subsequent production process. The high deformation rate deep pressing process of the alloy can be used during the rolling process to form a stable microstructure. The subsequent quenching and tight wire winding process is carried out in the low temperature zone. The dispersion amplitude inside the grain is smaller than that of other solutions, which is conducive to protecting the microstructure characteristics of the alloy wire.
[0034] Further or optionally, in the stretching deformation step S10, an ultra-precision stretching die is used, and the contact surface between the die and the metal rod to be stretched is provided with an ultra-fine particle coating to reduce the friction of the die on the alloy wire and maintain the smoothness of the surface.
[0035] In the wire drawing process, multiple dies are used for drawing, the wire drawing speed is controlled to be 8-18 m / s, and the deformation amount of each pass is controlled to be 15%-25%.
[0036] By adopting the above technical solution, the present invention has the following beneficial effects:
[0037] (1) The present application provides a high-conductivity ultra-high-strength aluminum alloy single wire, which uses multiple elements to synergistically improve the alloy performance based on the Mg2Si phase, controls the range of Mg / Si: = 0.92 to 1.25, promotes the evolution of the alloy grains into a highly uniform equiaxed grain structure, promotes the uniform distribution of grain boundaries, and thus enhances the comprehensive mechanical properties of the alloy material. It uses the high-temperature stable state of Al3Fe to limit the growth range of the crystal to prevent it from growing too long, adds titanium elements during the stirring process to increase the number of non-uniform nucleation points to promote stable crystal precipitation, uses Mg2Si phase to strengthen the alloy as a whole and prevent crystal phase dislocation, improves crystal regularity, uses copper elements to intervene in the solid solution and aging process of Al3Fe and Mg2Si phases, effectively prevents them from melting back, and ensures that the alloy continues to maintain its excellent performance after undergoing thermal cycles, and adds yttrium elements before alloy purification and casting to promote the formation of a dense oxide film on its surface, resist high-temperature oxidation, and enhance its internal thermal stability, preventing crystal phase damage caused by environmental exposure during subsequent processes.
[0038] (2) The present invention also provides a preparation process for a high-conductivity ultra-high-strength aluminum alloy single wire, which adopts a three-stage aging process and utilizes the synergistic effect between elements to effectively control the grain precipitation process inside the alloy. The alloy crystals have more crystallization nuclei, better grain regularity, and more stable precipitation. The dense oxide film formed by the synergistic effect of the yttrium element and the aluminum element inside can prevent the alloy from corroding in a harsh natural environment, so that the alloy aluminum wire achieves a balance between strength and conductivity.
[0039] (3) The present invention controls the refining temperature to 720°C to 740°C, which effectively prevents the alloy from excessively absorbing hydrogen and reduces the generation of bubbles. At the same time, it is beneficial to the full dissolution of alloy elements during the smelting process, effectively removes gas and inclusions, and reduces the situation of poor alloy performance. In this operation step, the refining agent is adjusted to 2.5:1000. At this ratio, a balance can be achieved between the refining agent cost and the amount of hydrogen escape, and the gas loss of the finished alloy is smaller.
[0040] (4) The present invention adopts a multi-layer foam ceramic filter plate and an external online removal system to realize a multi-level purification strategy, and finally achieves a deep-level double impurity removal effect, effectively improving the comprehensive performance and purity of the alloy rod; during its operation, high-purity nitrogen is used in coordination with the rotor to further remove gas impurities in the alloy.
[0041] (5) The present invention adopts a technology combining immersion water quenching and wind-blown air cooling during the rolling process. The temperature difference between the front and rear is large, which can achieve rapid cooling and block the process of grain expansion. The Al3Fe and boron-titanium-based components in the alloy work together to supply more crystal nuclei and limit the range of crystal growth, so that the alloy can obtain greater strength.
[0042] (6) The present invention adopts a step-by-step aging scheme to form a high-density micro-dispersed GP zone inside the alloy, providing abundant nucleation points for the subsequent precipitation phase, thus laying a foundation for the structural stability of the alloy; then, the final aging treatment is carried out under regulated high-temperature conditions, which not only avoids the solute remelting phenomenon, but also significantly improves the distribution uniformity of the precipitated phase.
[0043] (7) The present invention strictly controls the order of adding alloy raw materials and the alloy ratio, fully utilizing the fine modulation potential of each element on the microstructure of the aluminum alloy, and further improves the overall performance of the aluminum alloy by coordinating the subsequent staged aging treatment process.
[0044] (8) The rolling, quenching and tight wire winding processes of the present invention are performed in a low temperature zone, and the dispersion amplitude inside the grains is smaller than that of other solutions, which is beneficial to protecting the microstructural characteristics of the alloy wire.
[0045] (9) An ultra-precision drawing die is used in the alloy wire drawing process of the present invention, and an ultra-fine particle coating is provided on the contact surface between the die and the metal rod to be drawn to reduce the friction of the die on the alloy wire and maintain the surface smoothness. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments and in conjunction with the accompanying drawings, wherein
[0047] Figure 1 It is a schematic diagram of the structure of the present invention. DETAILED DESCRIPTION
[0048] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0049] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0050] All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without creative work shall fall within the protection scope of the present invention.
[0051] (Example 1)
[0052] A high-conductivity ultra-high-strength aluminum alloy single wire, whose chemical composition comprises the following components by weight: Fe 0.20%, Si 0.70%, Cu 0.025%, Mg 0.75%, B 0.005%, Ti 0.015%, Y 0.15%, Sc 0.05%, the remainder is Al, V+Cr≤0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0053] A production process for a high conductivity ultra-high strength aluminum alloy single wire as described above comprises the following steps:
[0054] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set to 760 degrees Celsius. Then, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, including 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additive, 8% aluminum boron (ALB 12 ) alloy, 10% aluminum yttrium alloy, 10% aluminum scandium alloy, and pure magnesium. During the process, an automatic stirring device is used for full and uniform mixing. The stirring lasts for 60 minutes to ensure the uniform distribution of each element. After the mixing is completed, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data feedback from the test, if necessary, the alloy ingredient ratio will be slightly adjusted, and the precise chemical composition will be fine-tuned again until the predetermined material performance requirements are met;
[0055] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0056] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0057] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0058] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 510℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0059] S6 online quenching: The hot-rolled aluminum alloy rod is kept at 340°C for online quenching and cooled to 65°C. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0060] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0061] S8 autonomous aging: The aluminum alloy rod is placed at room temperature for 168 hours to allow its internal structure to be fine-tuned and optimized spontaneously;
[0062] S9 stage aging: After the aluminum alloy wire has completed the aging in the autonomous state, it is transferred to a heat treatment chamber where the temperature is precisely controlled within the range of 110°C for 10 hours. The purpose is to promote the optimization and precipitation of the internal structure of the material through the primary stage of aging treatment, thereby enhancing its comprehensive mechanical properties;
[0063] S10 stretching deformation: The advanced high-speed aluminum alloy wire drawing machine is used for the stretching deformation process and the mold with precision-designed ultra-fine particle coating is used to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0064] S11 regulated aging: A continuous tunnel heat treatment furnace is used to apply a precise temperature-controlled aging process to the drawn aluminum alloy wire. The aging treatment temperature is 140°C and the duration is 12 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated to obtain a conductivity of ≥53.1% IACS, a tensile strength of ≥357MPa, and an elongation of ≥9.2%.
[0065] (Example 2)
[0066] A high-conductivity ultra-high-strength aluminum alloy single wire, whose chemical composition comprises the following components by weight: Fe 0.22%, Si 0.70%, Cu 0.03%, Mg 0.75%, B 0.005%, Ti 0.015%, Y 0.10%, Sc 0.08%, the remainder is Al, V+Cr≤0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0067] The production process includes the following steps:
[0068] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set to 760 degrees Celsius. Then, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, including 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additive, 8% aluminum boron (ALB 12 ) alloy, 10% aluminum yttrium alloy, 10% aluminum scandium alloy, and pure magnesium. During the process, an automatic stirring device is used for full and uniform mixing. The stirring lasts for 60 minutes to ensure the uniform distribution of each element. After the mixing is completed, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data feedback from the test, if necessary, the alloy ingredient ratio will be slightly adjusted, and the precise chemical composition will be fine-tuned again until the predetermined material performance requirements are met;
[0069] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0070] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0071] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0072] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 515℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0073] S6 online quenching: The temperature of the hot-rolled aluminum alloy rod is maintained at 355°C and rapidly cooled to 65°C through rapid cooling technology. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0074] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0075] S8 autonomous aging: The aluminum alloy rod is placed at room temperature for 240 hours to allow its internal structure to be fine-tuned and optimized spontaneously;
[0076] S9 stage aging: After the aluminum alloy wire has completed the aging in the autonomous state, it is transferred to a heat treatment chamber where the temperature is precisely controlled within the range of 130°C for 10 hours. The purpose is to promote the optimization and precipitation of the internal structure of the material through the primary stage of aging treatment, thereby enhancing its comprehensive mechanical properties;
[0077] S10 stretching deformation: The advanced high-speed aluminum alloy wire drawing machine is used for the stretching deformation process and the mold with precision-designed ultra-fine particle coating is used to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0078] S11 regulated aging: A continuous tunnel heat treatment furnace is used to apply a precise temperature-controlled aging process to the drawn aluminum alloy wire. The aging treatment temperature is 140°C and the duration is 12 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated to obtain a conductivity of ≥53.5% IACS, a tensile strength of ≥361MPa, and an elongation of ≥8.8%.
[0079] (Example 3)
[0080] A high-conductivity ultra-high-strength aluminum alloy single wire, whose chemical composition comprises the following components by weight: Fe 0.25%, Si 0.68%, Cu 0.025%, Mg 0.73%, B 0.005%, Ti 0.015%, Y 0.10%, Sc 0.11%, the remainder is Al, V+Cr≤0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0081] The production process includes the following steps:
[0082] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set to 760 degrees Celsius. Then, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, including 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additive, 8% aluminum boron (ALB 12 ) alloy, 10% aluminum yttrium alloy, 10% aluminum scandium alloy, and pure magnesium. During the process, an automatic stirring device is used for full and uniform mixing. The stirring lasts for 60 minutes to ensure the uniform distribution of each element. After the mixing is completed, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data feedback from the test, if necessary, the alloy ingredient ratio will be slightly adjusted, and the precise chemical composition will be fine-tuned again until the predetermined material performance requirements are met;
[0083] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0084] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0085] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0086] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 525℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0087] S6 online quenching: The temperature of the hot-rolled aluminum alloy rod is maintained at 375°C and rapidly cooled to 65°C through the above-mentioned rapid cooling technology. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0088] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0089] S8 autonomous aging: The aluminum alloy rod is placed at room temperature for 240 hours to allow its internal structure to be fine-tuned and optimized spontaneously;
[0090] S9 stage aging: After the aluminum alloy wire has completed the aging in the autonomous state, it is transferred to a heat treatment chamber where the temperature is precisely controlled within the range of 150°C for 10 hours. The purpose is to promote the optimization and precipitation of the internal structure of the material through the primary stage of aging treatment, thereby enhancing its comprehensive mechanical properties;
[0091] S10 stretching deformation: The advanced high-speed aluminum alloy wire drawing machine is used for the stretching deformation process and the mold with precision-designed ultra-fine particle coating is used to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0092] S11 regulated aging: A continuous tunnel heat treatment furnace is used to apply a precise temperature-controlled aging process to the drawn aluminum alloy wire. The aging treatment temperature is 120°C and the duration is 14 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated to obtain a conductivity of ≥54.5% IACS, a tensile strength of ≥372MPa, and an elongation of ≥6.6%.
[0093] (Example 4)
[0094] A high-conductivity ultra-high-strength aluminum alloy single wire, whose chemical composition comprises the following components by weight: Fe 0.20%, Si 0.65%, Cu 0.025%, Mg 0.70%, B 0.005%, Ti 0.012%, Y 0.10%, Sc 0.11%, the remainder is Al, V+Cr≤0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0095] The production process includes the following steps:
[0096] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set to 760 degrees Celsius. Then, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, including 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additive, 8% aluminum boron (ALB 12 ) alloy, 10% aluminum yttrium alloy, 10% aluminum scandium alloy, and pure magnesium. During the process, an automatic stirring device is used for full and uniform mixing. The stirring lasts for 60 minutes to ensure the uniform distribution of each element. After the mixing is completed, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data feedback from the test, if necessary, the alloy ingredient ratio will be slightly adjusted, and the precise chemical composition will be fine-tuned again until the predetermined material performance requirements are met;
[0097] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0098] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0099] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0100] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 520℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0101] S6 online quenching: The temperature of the hot-rolled aluminum alloy rod is maintained at 375°C and rapidly cooled to 65°C through rapid cooling technology. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0102] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0103] S8 autonomous aging: The aluminum alloy rod is placed at room temperature for 240 hours to allow its internal structure to be fine-tuned and optimized spontaneously;
[0104] S9 stage aging: After the aluminum alloy wire has completed the aging in the autonomous state, it is transferred to a heat treatment chamber where the temperature is precisely controlled within the range of 160°C for 8 hours. The purpose is to promote the optimization and precipitation of the internal structure of the material through the primary stage of aging treatment, thereby enhancing its comprehensive mechanical properties;
[0105] S10 stretching deformation: The advanced high-speed aluminum alloy wire drawing machine is used for the stretching deformation process and the mold with precision-designed ultra-fine particle coating is used to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0106] S11 regulated aging: A continuous tunnel heat treatment furnace is used to apply a precise temperature-controlled aging process to the drawn aluminum alloy wire. The aging treatment temperature is 120°C and the duration is 12 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated to obtain a conductivity of ≥54.7% IACS, a tensile strength of ≥363MPa, and an elongation of ≥6.6%.
[0107] (Comparative Example 1)
[0108] The chemical composition of the comparative case is: Fe 0.14%, Si 0.55%, Mg 0.75%, B 0.005%, Ti0.012%, RE0.15%, the balance is Al, V+Cr≤0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0109] The preparation process of the alloy wire comprises the following steps:
[0110] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set at 760 degrees Celsius. Then, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, including 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 10% aluminum-titanium alloy additive, 8% aluminum boron (ALB 12 ) alloy, 10% aluminum rare earth (RE) master alloy, pure magnesium, during which an automatic stirring device is used for full and uniform mixing, and the stirring lasts for 60 minutes to ensure the uniform distribution of each element. After mixing, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data feedback from the test, if necessary, the alloy ingredient ratio will be slightly adjusted, and the precise chemical composition will be fine-tuned again until the predetermined material performance requirements are met;
[0111] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0112] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0113] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0114] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 520℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0115] S6 online quenching: The temperature of the hot-rolled aluminum alloy rod is maintained at 375°C and rapidly cooled to 65°C through an efficient cooling technology. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0116] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0117] S8 Self-aging: The aluminum alloy rod is placed at room temperature and subjected to 240 hours of natural aging;
[0118] S9 stretching deformation: using advanced high-speed aluminum alloy wire drawing machine for stretching deformation process and using precision-designed ultra-fine particle coating mold, it aims to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0119] S11 regulated aging: artificial aging is applied to the aluminum alloy wire after drawing in a continuous tunnel heat treatment furnace, with an aging temperature of 160°C and a duration of 8 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated to obtain a conductivity of ≥53.3%IACS, a tensile strength of ≥319MPa, and an elongation of ≥6.2%.
[0120] (Comparative Example 2)
[0121] The chemical composition is the same as that of comparative case 1: Fe 0.14%, Si 0.55%, Mg 0.75%, B 0.005%, Ti0.012%, RE0.15%, the balance is Al, V+Cr≤0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0122] The preparation process of the alloy wire comprises the following steps:
[0123] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set to 760 degrees Celsius. Then, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, including 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 10% aluminum-titanium alloy additives, 8% aluminum-boron (ALB12) alloy, 10% aluminum rare earth (RE) master alloy, and pure magnesium. During this period, an automatic stirring device is used for full and uniform mixing. The stirring lasts for 60 minutes to ensure the uniform distribution of each element. After mixing, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data feedback from the test, if necessary, the alloy ingredient ratio will be slightly adjusted, and the precise chemical composition will be fine-tuned again until the predetermined material performance requirements are met;
[0124] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0125] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0126] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0127] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 520℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0128] S6 online quenching: The temperature of the hot-rolled aluminum alloy rod is maintained at 375°C and rapidly cooled to 65°C through an efficient cooling technology. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0129] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0130] S8 autonomous aging: The aluminum alloy rod is placed at room temperature for 240 hours to allow its internal structure to be fine-tuned and optimized spontaneously;
[0131] S9 stage aging: After the aluminum alloy wire has completed the aging in the autonomous state, it is transferred to a heat treatment chamber where the temperature is precisely controlled within the range of 160°C for 8 hours. The purpose is to promote the optimization and precipitation of the internal structure of the material through the primary stage of aging treatment, thereby enhancing its comprehensive mechanical properties;
[0132] S10 stretching deformation: The advanced high-speed aluminum alloy wire drawing machine is used for the stretching deformation process and the mold with precision-designed ultra-fine particle coating is used to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0133] S11 regulated aging: A continuous tunnel heat treatment furnace is used to apply a precise temperature-controlled aging process to the aluminum alloy wire after drawing. The aging treatment temperature is 120°C and the duration is 12 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated.
[0134] The obtained conductivity is ≥54.4% IACS, the tensile strength is ≥348 MPa, and the elongation is ≥5.2%.
[0135] (Comparative Example 3)
[0136] The chemical composition is the same as that of Case 4: Fe 0.20%, Si 0.65%, Cu 0.025%, Mg 0.70%, B 0.005%, Ti 0.012%, Y 0.10%, Sc 0.11%, the remainder is Al, V+Cr ≤ 0.005%, and the rest is aluminum (Al) and other inevitable trace impurity elements.
[0137] The preparation process of the alloy wire comprises the following steps:
[0138] S1 Melting: First, the remelted aluminum block with a purity of 99.70% is melted into liquid. Subsequently, the aluminum liquid is introduced into a tilting holding furnace with a loading capacity of 10 tons, which is equipped with an advanced magnetic-driven automatic stirring system. The temperature in the furnace is set to 760 degrees Celsius. Next, a series of pre-proportioned alloying elements are added to the aluminum liquid in steps, covering 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additives, 8% aluminum-boron (ALB12) alloy, 10% aluminum-yttrium alloy, 10% aluminum-scandium alloy, and pure magnesium. During this period, an automatic stirring device is used for full and uniform mixing, and the stirring lasts for 60 minutes to ensure the uniform distribution of each element. After mixing, the aluminum alloy liquid is immediately tested for its chemical composition. Based on the detailed data from the test, if necessary, the alloy proportions are fine-tuned and the chemical composition is fine-tuned again until the predetermined material performance requirements are met.
[0139] S2 refining: The refining agent is introduced at a temperature of 730 degrees Celsius to ensure that the mass ratio of the refining agent to the aluminum alloy melt is kept near the general optimization ratio, which is about 2.5 units of refining agent for every 1000 units of aluminum alloy melt. The refining operation lasts for 35 minutes to fully optimize the purity of the melt. In addition, after the refining is completed, the melt is placed in a stable temperature range and kept at 740 degrees Celsius for a period of 30 minutes;
[0140] S3 purification and grain optimization: The aluminum alloy melt is injected into the rotor-driven degassing chamber through a special inlet. At the same time, a grain refiner of 0.25‰ of the total amount of the aluminum alloy solution is blended at the inlet, and the titanium boron and rare earth elements are 5Ti1B1RE. Combined with the coordinated action of high-purity nitrogen and the rotor, the residual hydrogen in the melt is efficiently removed, and the penetration of additives is purified and optimized. After that, the melt is transferred to a precisely temperature-controlled constant temperature chamber to ensure a uniform and stable temperature of the melt at a constant temperature of 740°C. Next, the melt passes through a ceramic filter chamber, which is equipped with a special ion interception ceramic plate with an aperture (40ppi / 50ppi) to effectively filter out harmful impurities and deepen purity assurance. After filtration, the melt is smoothly discharged from the lower port and then led to the casting equipment;
[0141] S4 continuous casting: The specially treated aluminum alloy melt flows smoothly to the casting equipment through an optimized flow guide system. The aluminum alloy melt is accurately guided into the crystallizer in a continuous flow state. The casting speed is set to 5.5 tons per hour and the cooling water temperature is controlled at 28°C. Continuous direct solidification is achieved to form the initial form of the aluminum alloy ingot;
[0142] S5 continuous hot rolling: The aluminum alloy ingot is first guided to the heating equipment, and the temperature is adjusted to 520℃ through a precise temperature management system. After reaching the required temperature, the aluminum alloy ingot quickly enters the continuous rolling process. This process uses rough rolling and finishing rolling equipment in series. After preliminary processing in the rough rolling mill and careful adjustment in the finishing mill, an aluminum alloy rod with a diameter of 9.5mm is finally produced;
[0143] S6 online quenching: The temperature of the hot-rolled aluminum alloy rod is maintained at 375°C and rapidly cooled to 65°C through an efficient cooling technology. This cooling method is designed to ensure that the aluminum alloy rod is completely transformed into a supersaturated solid solution state to achieve a specific heat treatment effect. The process focuses on achieving rapid and uniform cooling to optimize the microstructure and macroscopic properties of the material;
[0144] S7 Tight Winding: It uses an advanced automation system to complete the winding of the aluminum alloy rod. This system can wind the aluminum alloy rod after it cools to 60℃. In addition, through precise control technology, it ensures that the weight of each roll of aluminum alloy rod is kept at around 2500kg.
[0145] S8 autonomous aging: The aluminum alloy rod is placed at room temperature for 240 hours to allow its internal structure to be fine-tuned and optimized spontaneously;
[0146] S9 stretching deformation: using advanced high-speed aluminum alloy wire drawing machine for stretching deformation process and using precision-designed ultra-fine particle coating mold, it aims to significantly reduce the friction resistance during the deformation process and ensure the surface smoothness and gloss of the finished product. By adopting multi-stage continuous molding technology, the balanced optimization of the material microstructure is achieved, ensuring the consistency and uniformity of the internal organization;
[0147] S10 regulated aging: A continuous tunnel heat treatment furnace is used to apply a precise temperature-controlled aging process to the aluminum alloy wire after drawing. The aging treatment temperature is 160°C and the duration is 8 hours. The phase change process and crystal structure rearrangement inside the aluminum alloy are regulated.
[0148] The obtained conductivity is ≥53.6% IACS, the tensile strength is ≥341 MPa, and the elongation is ≥6.2%.
[0149] The samples obtained in the above embodiments and comparative examples were tested, and the obtained parameters are shown in the following table:
[0150] Table 1 Performance comparison between common alloy wire and alloy wire of the present invention
[0151]
[0152] Through comparative analysis, we found that in addition to the basic elements of magnesium (Mg) and silicon (Si), the introduction of trace elements has a significant effect on the properties of the alloy. In particular, the addition of copper (Cu), yttrium (Y) and scandium (Sc) not only improves the microstructure of the alloy, but also significantly improves its macroscopic properties. First, the introduction of Sc improves the precipitation behavior of Cu and promotes the formation of a finer and more evenly distributed Cu-Sc co-precipitation phase. This change directly improves the hardness and strength of the alloy. In addition, the composite Al-Sc-Y phase formed by Sc and Y further improves the overall performance of the alloy due to its better strengthening effect.
[0153] In terms of microstructure control of the alloy, through staged aging treatment and precise aging control, we have successfully guided the microstructure of the alloy to a uniform equiaxed crystal morphology. This structural transformation not only optimizes the distribution of grain boundaries, but also significantly improves the mechanical properties of the alloy, achieving an excellent balance of strength, conductivity and ductility.
[0154] In addition, this study innovatively applied the combination of trace elements and aging process to promote the massive formation and orderly arrangement of β" phase cores. The dense distribution of these cores on the grain boundaries greatly increased the nucleation points and accelerated the diffusion rate of impurity elements. This process effectively reduced the size of the precipitation-free zone, further refined the microstructure of the material, and provided a new way to comprehensively improve the performance of aluminum alloy materials.
[0155] Through refined alloy composition design and innovative processing technology, we have not only achieved a significant leap in alloy performance, but also opened up new possibilities for the application and development of aluminum alloy materials.
[0156] It should be understood that the present invention is described by some embodiments, and those skilled in the art will appreciate that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application belong to the scope of protection of the present invention.
Claims
1. A high conductivity and ultra-high strength aluminum alloy single wire, It is characterized in that Its composition is 0.60%~0.80% silicon, 0.65%~0.85% magnesium, 0.14%~0.25% iron, 0.05%~0.15% scandium, 0.01%~0.03% copper, 0.01%~0.15% yttrium, 0.001%~0.015% titanium, V+Cr≤0.005%, and the rest is aluminum and other inevitable trace impurity elements.
2. A process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 1, Features The steps include: S1 smelting: smelting aluminum ingots and master alloy ingots according to a predetermined chemical ratio; S2 refining: After smelting, the material is transferred to a holding furnace for deep purification to obtain aluminum alloy melt; S3 purification and grain optimization: The aluminum alloy melt is transferred into the dynamic purification system, and then the grains are refined and high-precision considered; S4 continuous casting: The alloy liquid after grain optimization is introduced into the casting device, and the aluminum alloy ingot blank is prepared by horizontal continuous casting: S5 continuous hot rolling: the aluminum alloy ingot is sent into the temperature control heating system and then evenly heated, and then continuously hot rolled to obtain the alloy rod; S6 online quenching: rapid cooling of the alloy rod; S7 closes the line tightly; S8 Self-aging: The alloy rod after winding is placed at room temperature for self-aging; S9 stage aging: the alloy rod after self-aging is placed in the aging furnace for stage aging treatment; S10 tensile deformation: tensile deformation treatment is performed on the alloy rod that has completed stage aging; S11 regulatory timeliness.
3. A process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features: In the S2 refining step, the refining operation range is 720°C to 740°C, the refining time is 30 to 45 minutes, the ratio of refining agent to aluminum alloy solution is 2.5:1000, and then the temperature is kept at 730°C to 760°C for 25 minutes.
4. The process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features: In the S3 purification and grain optimization step, the purification system uses a multi-layer foam ceramic filter plate with a pore size range of 40ppi to 50ppi, a filtration temperature of 740°C, a total amount of 0.25% grain optimizer, and a titanium boron rare earth refiner. High-purity nitrogen is used in the purification process in coordination with the rotor.
5. The process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features The temperature of the thermostatic heating in the S5 continuous rolling step is 505°C-535°C, the quenching temperature in the S6 online quenching step is 28°C-30°C, and the quenching pressure is 500±50kpa. During the quenching process, immersion water cooling is performed first, and then air cooling is performed.
6. The process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features The S8 autonomous aging step condition is room temperature, and the aging time is not less than 168 hours; the S9 staged aging condition is 110°C to 160°C, and the aging time is 8 to 24 hours; the step S11 regulatory aging step condition is a temperature of 120°C to 160°C, and the aging time is 5 to 15 hours.
7. The process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features In the S1 smelting step, the alloy ingot used has an aluminum alloy purity of ≥99.70%, a magnetically driven automatic stirring system is used, the furnace temperature is 750-760°C, and the alloy adding components and steps are 10% aluminum-iron master alloy, 10% aluminum-silicon alloy, 50% aluminum-copper alloy, 10% aluminum-titanium alloy additive, 8% aluminum-boron (ALB12) alloy, 10% aluminum-yttrium alloy, 10% aluminum-scandium alloy, and pure magnesium.
8. The process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features In the S5 continuous hot rolling step, the hot rolling completion temperature is ≥360°C, in the S6 online quenching step, the cooling temperature is 65°C to 110°C, and in the S7 tight wire winding step, the wire winding temperature is ≤100°C.
9. The process for preparing a high conductivity ultra-high strength aluminum alloy single wire according to claim 2, Features In the stretching deformation step S10, an ultra-precision stretching die is used, and the contact surface between the die and the metal rod to be stretched is provided with an ultra-fine particle coating.
Citation Information
Cited By
Preparation method of aluminum-based enameled wire for automobile
CN120126865A