Large-thickness low-temperature-toughness high-strength Q690E steel plate and production process thereof

Through specific chemical composition and production process design, the problem of high yield strength and low-temperature impact toughness of high-thick Q690E grade steel plates in the existing technology is solved, and high-efficiency production of high-performance 120mm thickness steel plates is achieved to meet the material design of engineering machinery. Standard and reduce production costs.

CN118979204APending Publication Date: 2024-11-19NANJING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105997.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

It is difficult to develop high-thickness Q690E grade steel plates with high yield strength and low temperature impact toughness in the prior art, and the existing production process is inefficient, which cannot meet the strict requirements of engineering machinery for high-strength steel plates and the continuous demand of industrial production.

Method used

Using specific chemical composition design and production processes, including molten iron pretreatment, converter smelting, LF refining, RH refining, continuous casting, rolling and heat treatment, ensure high strength of the steel plate by controlling carbon content, alloy element addition and tempering heat treatment. and low-temperature impact toughness, and through two-stage controlled rolling and reasonable temperature control of casting billets, ensuring the uniformity and performance of the steel plate.

Benefits of technology

The production of high-strength steel plate with a thickness of 120mm was achieved, with yield strength ≥650MPa, tensile strength meeting 710~900MPa, elongation ≥14%, longitudinal impact work ≥50J in -40℃, Z-directional performance >35%, and production was shortened at the same time Cycles and reduce costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979204A_ABST
    Figure CN118979204A_ABST
Patent Text Reader

Abstract

The invention discloses a large-thickness low-temperature-toughness high-strength Q690E steel plate and a production process thereof, and relates to the technical field of steel production, and the large-thickness low-temperature-toughness high-strength Q690E steel plate comprises the following chemical components in percentage by mass: 0.16 to 0.18 percent of C, 1.10 to 1.20 percent of Mn, 0.20 to 0.30 percent of Si, 0.43 to 0.50 percent of Cr, 0.45 to 0.50 percent of Mo, 0.90 to 1.10 percent of Ni, 0.015 to 0.025 percent of Nb, 0.030 to 0.040 percent of V, less than or equal to 0.010 percent of Ti, 0.025 to 0.055 percent of Alt, 0.0012 to 0.0020 percent of Bt, 0.0008 to 0.0030 percent of Ca, less than or equal to 0.008 percent of P, less than or equal to 0.002 percent of The high-strength steel with the thickness reaching 120mm is produced by adopting a reasonable control process, and the performance meets the standard requirements of engineering machinery on material design by using an optimal quenching and tempering heat treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, and in particular to a thick, low-temperature toughness, high-strength Q690E steel plate and a production process thereof. Background Art

[0002] Low-alloy wide and thick steel plates with high strength are widely used in the manufacturing industries of engineering machinery, mining machinery, vehicle structures, containers, etc. With the increasing size and efficiency of engineering machinery, the demand for further development of wide and thick steel plates with higher yield strength and low-temperature impact toughness is becoming stronger. At the same time, the service conditions of engineering machinery are becoming more and more harsh, so higher requirements are also placed on the toughness and plasticity of steel plates. Especially in specific working conditions and fields, for wide and thick plates with a thickness of 120mm, the shrinkage requirements of the entire thickness section of the steel plate are extremely strict.

[0003] Patent CN109988968A discloses a low-carbon equivalent thick Q690E grade high-strength steel plate and its production method. The method uses a 330mm thick ingot, a product thickness of 110mm and ensures that the various properties of the steel plate meet the requirements, but does not describe the performance of a 120mm thick steel plate.

[0004] Patent CN109234632A discloses 80-120 thick easy-to-weld corrosion-resistant high-strength Q690E steel plates for deep-sea submarines and their production methods. The patent adopts water-cooled mold casting, and the production process is cumbersome, the production time is long and the efficiency is low, which cannot meet the continuous production needs.

[0005] From the above analysis, it can be seen that there are currently very few patents involving the development of steel plates with a yield strength of Q690MPa, a thickness of 120mm and good low-temperature impact toughness. However, under the demand for large-scale development of certain specific equipment in the field of engineering machinery, it is particularly important to ensure the safe service performance of thick high-strength steel plates and good low-temperature impact toughness. Secondly, improving industrial production efficiency and reducing costs are also crucial. Therefore, it is necessary to develop a thick, high-strength, low-temperature impact toughness steel. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a thick low-temperature toughness high-strength Q690E steel plate and a production process thereof.

[0007] In order to solve the above technical problems, the technical solution of the present invention is as follows: A thick low-temperature toughness and high-strength Q690E steel plate, whose chemical composition and mass percentage are as follows: C: 0.16-0.18%, Mn: 1.10-1.20%, Si: 0.20-0.30%, Cr: 0.43-0.50%, Mo: 0.45-0.50%, Ni: 0.90-1.10%, Nb: 0.015-0.025%, V: 0.030-0.040%, Ti: ≤0.010%, Alt: 0.025-0.055%, Bt: 0.0012-0.0020%, Ca: 0.0008-0.0030%, P≤0.008%, S≤0.002%, N≤0.0055%, H≤0.00018%, and the balance is iron and unavoidable impurities.

[0008] The present invention also provides a production process for a thick, low-temperature toughness, high-strength Q690E steel plate, which comprises in sequence: molten iron pretreatment, converter smelting, LF refining, RH refining, continuous casting, rolling and heat treatment.

[0009] As a preferred solution of the production process of the thick low-temperature toughness and high-strength Q690E steel plate described in the present invention, the molten iron pretreatment includes: using the KR method or the blowing method to perform molten iron pretreatment desulfurization, and performing slag removal treatment.

[0010] As a preferred solution of the production process of the thick low-temperature toughness and high-strength Q690E steel plate described in the present invention, the mass fraction of S in the molten iron after the molten iron pretreatment is ≤0.0020%.

[0011] As a preferred solution of the production process of the thick low-temperature toughness and high-strength Q690E steel plate of the present invention, the converter smelting includes: The top and bottom combined blowing converter is used for decarburization, desiliconization and desulfurization of molten iron, and the tapping temperature is controlled at 1600-1630℃; After the steel is tapped from the converter, aluminum is added for deoxidation so that the mass fraction of total oxygen in the molten steel is ≤0.0500%, and 5.2±0.3kg / t of lime and 2.3±0.3kg / t of pre-melted refined slag are added during the tapping process.

[0012] As a preferred solution of the production process of the thick low-temperature toughness high-strength Q690E steel plate of the present invention, the LF refining comprises: Add lime and fluorite to the LF refining furnace to control the basicity to 4.5-6.5; Aluminum is used for deoxidation to make the mass fraction of total oxygen in the molten steel ≤0.0020% and the mass fraction of dissolved oxygen ≤0.0005%.

[0013] As a preferred solution of the production process of the thick low-temperature toughness high-strength Q690E steel plate of the present invention, the RH refining includes: Control the vacuum degree of RH refining furnace ≤3.0mbar and the duration ≥25min; After RH refining, boron is added and calcium treatment is carried out. After calcium treatment, the static stirring time is ≥15min.

[0014] As a preferred solution of the production process of the thick low temperature toughness high strength Q690E steel plate of the present invention, the continuous casting comprises: The tundish uses carbon-free covering agent, medium carbon steel protective slag is used for casting, and the temperature of the molten steel in the tundish is controlled at 10-20℃.

[0015] As a preferred solution of the production process of the thick low temperature toughness high strength Q690E steel plate of the present invention, the rolling comprises: When the continuous casting billet is above 150℃, it is heated into the furnace, the heating temperature is 1150±20℃, the heating time is 9~17min / cm, and the soaking time is 1.4min / cm; Two-stage controlled rolling is adopted, with the starting rolling temperature of 1130±20℃ in the first stage and the target final rolling temperature of 840±20℃, followed by air cooling after rolling.

[0016] As a preferred solution of the production process of the thick low-temperature toughness high-strength Q690E steel plate of the present invention, the heat treatment comprises: The quenching heating temperature is 910±10℃, the heating rate is 1.5±0.1min / mm, and the time in the furnace is 170~200min; the tempering heating temperature is 650±10℃, the heating rate is 2.5±0.1min / mm, the time in the furnace is 330~350min, and then slowly cooled to room temperature.

[0017] The beneficial effects of the present invention are: (1) The present invention adopts a medium carbon component design, adds trace amounts of alloying elements Cr, Ni, and V, and has a carbon equivalent of ≤0.63%, a short production cycle, and low cost.

[0018] (2) The present invention adopts a reasonable control process to produce high-strength steel with a thickness of 120 mm and uses the optimal tempering heat treatment process so that the performance meets the standard requirements of engineering machinery for material design, with a yield strength of ≥650 MPa, a tensile strength of 710 to 900 MPa, an elongation of ≥14%, a longitudinal impact energy of ≥50 J at -40°C, and Z-direction performance of >35%.

[0019] (3) Due to the high strength requirement, the present invention adopts a large reduction mode for controlled rolling, uses a 320 mm thick ingot, controls the soaking temperature at 1150°C, and appropriately prolongs the furnace time to ensure uniform ingot steel temperature.

[0020] (4) The thickness of the product of the present invention is 120 mm. In order to avoid core segregation during the rolling process, which affects the mechanical properties and low-temperature impact toughness, the cumulative reduction rates in the two stages are ensured to be 60% and 70%, respectively, to ensure that there is no obvious difference between the surface and core structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0022] Figure 1 This is a metallographic diagram of a thick, low-temperature toughness, high-strength Q690E steel plate prepared in Example 1; Figure 2 This is a metallographic diagram of the thick, low-temperature toughness, high-strength Q690E steel plate prepared in Example 2. DETAILED DESCRIPTION

[0023] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.

[0024] The present application provides a large thickness, low-temperature toughness, high-strength Q690E steel plate, whose chemical composition and mass percentage are as follows: C: 0.16-0.18%, Mn: 1.10-1.20%, Si: 0.20-0.30%, Cr: 0.43-0.50%, Mo: 0.45-0.50%, Ni: 0.90-1.10%, Nb: 0.015-0.025%, V: 0.030-0.040%, Ti: ≤0.010%, Alt: 0.025-0.055%, Bt: 0.0012-0.0020%, Ca: 0.0008-0.0030%, P≤0.008%, S≤0.002%, N≤0.0055%, H≤0.00018%, and the balance is iron and unavoidable impurities.

[0025] The present application also provides a production process for a thick low-temperature toughness high-strength Q690E steel plate, which comprises the following steps: Step S101: molten iron pretreatment: The molten iron is pretreated and desulfurized by the KR method or the injection method. The molten iron is slag-scraped after the pretreatment to ensure that the mass fraction of S in the molten iron is ≤0.0020%.

[0026] Step S102: Converter smelting: Use a top and bottom double-blown converter to decarburize, desiliconize and desulfurize molten iron, and control the tapping temperature at 1600-1630°C. Add aluminum for deoxidation after the converter tapping, and control the mass fraction of total oxygen in the molten steel to ≤0.0500%. Add 5.2±0.3kg / t of lime and 2.3±0.3kg / t of pre-melted refined slag during the tapping process.

[0027] It should be noted that lime 5.2±0.3kg / t steel and pre-melted refined slag 2.3±0.3kg / t steel are mainly a mixture of CaO and SiO2, in order to increase the basicity of molten steel.

[0028] Step S103: LF refining: lime and fluorite are added appropriately according to the slag conditions, and the basicity is controlled at 4.5-6.5. Aluminum particles / aluminum powder / aluminum wire are used for deoxidation, and the mass fraction of total oxygen in the molten steel is controlled to be ≤0.0020%, and the mass fraction of dissolved oxygen is ≤0.0005%.

[0029] Step S104: RH refining: The RH refining furnace is placed in a high vacuum (≤3.0 mbar) and maintained for ≥25 min. After the RH refining is completed, ferroboron is added or boron wire is fed, and then seamless pure calcium wire, silicon calcium wire or pure calcium wire is fed. After the calcium treatment is completed, the static stirring time is ≥15 min.

[0030] Step S105: Continuous casting: The long nozzle and the submerged nozzle of continuous casting are strictly sealed with argon, the casting speed is controlled within a reasonable range, the tundish adopts a carbon-free covering agent, the casting adopts a medium carbon steel protective slag, and the temperature of the molten steel in the tundish is controlled within the range of 10-20°C.

[0031] Step S106: Rolling: The continuous casting billet is heated to above 150°C and is heated by covering the bottom with a cover or preheating in a tabletop furnace. The heating temperature is 1150±20°C. The heating time and soaking time are calculated according to the thickness of the billet. The heating time is 9-17min / cm, and the soaking time is 1.4min / cm. The rolling is carried out in two stages. The first stage rolling temperature is 1130±20°C, the target final rolling temperature is 840±20°C, and the rolling is air-cooled. The cumulative reduction rates of the two stages are 60% and 70% respectively.

[0032] Step S107: Heat treatment: quenching heating temperature is 910±10℃, heating rate is 1.5±0.1min / mm, and time in the furnace is 170-200min; tempering heating temperature is 650±10℃, heating rate is 2.5±0.1min / mm, and time in the furnace is 330-350min, and then slowly cooled to room temperature.

[0033] The above technical solution is described below through specific embodiments.

[0034] Example 1: The target steel plate thickness specification obtained in this example is 120 mm. The chemical composition and mass percentage of the steel are as follows: C: 0.178 wt.%, Si: 0.23 wt.%, Mn: 1.13 wt.%, P: 0.007 wt.%, S: 0.002 wt.%, Cr: 0.45 wt.%, V: 0.032 wt.%, CE carbon equivalent 0.62.

[0035] When preparing the above-mentioned target steel plate, after converter steelmaking alloying and deoxidation, LF + RH refining and continuous casting are performed, the billet is heated at 1150°C, the starting rolling temperature is 1130°C, the final rolling temperature is 840°C, the quenching temperature is controlled at 905°C, the heating rate is 1.5min / mm, the furnace time is 195min, the tempering temperature is controlled at 650°C, the heating rate is 2.5min / mm, the furnace time is 350min, and it is slowly cooled to room temperature.

[0036] Example 2: The target steel plate thickness specification obtained in this example is 120 mm. The chemical composition and mass percentage of the steel are as follows: C: 0.173 wt.%, Si: 0.25 wt.%, Mn: 1.15 wt.%, P: 0.007 wt.%, S: 0.001 wt.%, Cr: 0.46 wt.%, V: 0.038 wt.%, CE carbon equivalent 0.62.

[0037] When preparing the above-mentioned target steel plate, after converter steelmaking alloying and deoxidation, LF + RH refining and continuous casting are performed, the billet is heated to 1160°C, the starting rolling temperature is 1150°C, the final rolling temperature is 850°C, the quenching temperature is controlled at 910°C, the heating rate is 1.4 min / mm, the furnace time is 183 min, the tempering temperature is controlled at 660°C, the heating rate is 2.6 min / mm, the furnace time is 240 min, and it is slowly cooled to room temperature.

[0038] The thick, low-temperature toughness, high-strength Q690E steel plates prepared in Examples 1 and 2 are shown in Table 1.

[0039]

[0040] Table 1 It can be seen from Table 1 that the strength of the thick low-temperature toughness and high-strength Q690E steel plates prepared in Examples 1 and 2 meets the use requirements, the low-temperature -40°C longitudinal impact toughness is stable and excellent, and has high strength and toughness.

[0041] Therefore, the technical solution of this application adopts a medium carbon component design, adding trace amounts of alloying elements Cr, Ni, and V, with a carbon equivalent of ≤0.63%, a short production cycle, and low cost. At the same time, a reasonable control process is used to produce high-strength steel with a thickness of 120mm, and the optimal quenching and tempering heat treatment process is used to make the performance meet the standard requirements of engineering machinery for material design, with a yield strength of ≥650MPa, a tensile strength of 710-900MPa, an elongation of ≥14%, a longitudinal impact energy of ≥50J at -40℃, and Z-direction performance of >35%.

[0042] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.

Claims

1. A thick low temperature toughness high strength Q690E steel plate, Features: Its chemical composition and mass percentage are as follows: C: 0.16-0.18%, Mn: 1.10-1.20%, Si: 0.20-0.30%, Cr: 0.43-0.50%, Mo: 0.45-0.50%, Ni: 0.90-1.10%, Nb: 0.015-0.025%, V: 0.030-0.040%, Ti: ≤0.010%, Alt: 0.025-0.055%, Bt: 0.0012-0.0020%, Ca: 0.0008-0.0030%, P≤0.008%, S≤0.002%, N≤0.0055%, H≤0.00018%, and the balance is iron and unavoidable impurities.

2. A production process for the thick, low-temperature toughness, high-strength Q690E steel plate according to claim 1, Features: Including in order: Hot metal pretreatment, converter smelting, LF refining, RH refining, continuous casting, rolling and heat treatment.

3. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The molten iron pretreatment includes: using the KR method or the injection method to perform molten iron pretreatment desulfurization, and performing slag removal treatment.

4. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 3, Features: The mass fraction of S in the molten iron after the molten iron pretreatment is ≤0.0020%.

5. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The converter smelting comprises: The top and bottom combined blowing converter is used for decarburization, desiliconization and desulfurization of molten iron, and the tapping temperature is controlled at 1600-1630℃; After the steel is tapped from the converter, aluminum is added for deoxidation so that the mass fraction of total oxygen in the molten steel is ≤0.0500%, and 5.2±0.3kg / t of lime and 2.3±0.3kg / t of pre-melted refined slag are added during the tapping process.

6. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The LF refining includes: Add lime and fluorite to the LF refining furnace to control the basicity to 4.5-6.5; Aluminum is used for deoxidation to make the mass fraction of total oxygen in the molten steel ≤0.0020% and the mass fraction of dissolved oxygen ≤0.0005%.

7. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The RH refining includes: Control the vacuum degree of RH refining furnace ≤3.0mbar and the duration ≥25min; After RH refining, boron is added and calcium treatment is carried out. After calcium treatment, the static stirring time is ≥15min.

8. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The continuous casting comprises: The tundish uses carbon-free covering agent, medium carbon steel protective slag is used for casting, and the temperature of the molten steel in the tundish is controlled at 10-20℃.

9. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The rolling comprises: When the continuous casting billet is above 150℃, it is heated into the furnace, the heating temperature is 1150±20℃, the heating time is 9~17min / cm, and the soaking time is 1.4min / cm; Two-stage controlled rolling is adopted, with the starting rolling temperature of 1130±20℃ in the first stage and the target final rolling temperature of 840±20℃, followed by air cooling after rolling.

10. The production process of the thick low-temperature toughness high-strength Q690E steel plate according to claim 1, Features: The heat treatment comprises: The quenching heating temperature is 910±10℃, the heating rate is 1.5±0.1min / mm, and the time in the furnace is 170~200min; the tempering heating temperature is 650±10℃, the heating rate is 2.5±0.1min / mm, the time in the furnace is 330~350min, and then slowly cooled to room temperature.