Preparation method and system of lead alloy composite anode with 3D porous structure
By introducing 3D porous structure and composite plating design into the lead alloy anode, the problems of unstable performance and complex preparation processes of traditional anode are solved, and efficient electrochemical performance and corrosion resistance are achieved, which are suitable for electrolysis and electroplating processes.
Patent Information
- Application Number
- CN202411039463.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional lead alloy anodes have problems such as high density, poor mechanical properties, low conductivity and high oxygen evolution overpotential, which leads to difficult operation and high power consumption. The preparation process of porous anodes is complex and costly, making it difficult to obtain uniform pore distribution. product.
Using the preparation method of 3D porous structure lead alloy composite anode, the lead alloy and foam copper foam are treated in a mixed sodium salt solution, and a three-dimensional through-pore structure is formed using a hot pressing furnace, followed by constant current polarization in the sulfuric acid electrolyte. Finally, PbO2-WC plating and Co3O4 plating were applied to the 3D lead alloy substrate, and a dense Co3O4 plating was formed by radio frequency magnetron sputtering.
It significantly improves the corrosion resistance and electrochemical properties of the anode, extends the service life, reduces the overpotential of the oxygen evolution reaction, and improves the electrochemical reaction efficiency. It is suitable for batteries and electrolytic cells and other fields.
Smart Images

Figure CN118979289A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of Pb anode materials, and in particular relates to a preparation method and system for a 3D porous structure lead alloy composite anode. Background Art
[0002] The extraction methods of heavy metals such as copper, zinc, manganese, nickel and cobalt can be roughly divided into two types: pyrometallurgy and hydrometallurgy. Hydrometallurgy has the advantages of high comprehensive recovery rate of valuable metals, low degree of air pollution, strong adaptability to low-grade ores and easy automation of production process, and its share in the mining of these non-ferrous metals is gradually increasing. For example, nearly 20% of the world's copper production capacity, more than 85% of zinc, most of manganese, and almost 100% of high-purity nickel and cobalt are extracted by hydrometallurgy.
[0003] In the hydrometallurgical process, electrodeposition is a crucial process, and lead alloy flat plates are usually used as insoluble anodes. However, the traditional lead alloy flat plate anode has the disadvantages of high density, poor mechanical properties, low conductivity, and high oxygen evolution overpotential, which leads to difficult anode operation and high power consumption. Domestic and foreign researchers have actively explored it and made a lot of progress. Among them, the porous anode has a higher exchange current density, lower charge transfer resistance and oxygen evolution overpotential compared with the traditional lead alloy anode due to the increase in actual surface area. The known preparation methods of porous lead anodes are infiltration casting and powder metallurgy. The principle of infiltration casting is: first, the pre-treated filler particles are directly placed in the mold, and preheated together with the mold to a certain temperature; then pour in molten metal lead and apply appropriate pressure to make the metal lead liquid penetrate into the gaps of the filler particles; after cooling and solidification, the filler particles are removed by appropriate methods to obtain a porous lead alloy. The advantages of infiltration casting are simple process and uniform pore structure; the disadvantage is that some filler particles are easily coated by the lead alloy liquid to form closed pores. These filler particles will be retained in the closed pores and cannot be removed, and gradually corrode the anode. This will not only affect the performance, but also cause adverse consequences. The principle of powder metallurgy is: mix the lead alloy powder with an appropriate amount of foaming agent powder evenly, press it into a preform with a certain density under appropriate pressure; then put it into the mold for heating treatment to decompose the foaming agent, release gas to expand the preform, and form a porous lead alloy. The porous lead alloy prepared by powder metallurgy is of high quality and stable performance. However, the preparation process of powder metallurgy is relatively complicated, the production cost is high, and the foaming process is difficult to control, so it is difficult to obtain a product with uniform pore distribution.
[0004] Porous anodes have the problem of reduced service life, so WC and Co3O4 coatings are applied to the surface of 3D lead alloy to improve the corrosion resistance of the anode and further increase the electrochemical properties of the anode. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a method and system for preparing a 3D porous structure lead alloy composite anode.
[0006] The present invention is achieved by a method for preparing a 3D porous structure lead alloy composite anode, the method comprising:
[0007] S1: Cut the lead alloy plate and the foam copper plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and foam copper in a prepared mixed sodium salt solution (20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, 20g / L sodium phosphate), soak for 3 minutes to remove oil stains on the surface of the foam aluminum, rinse with distilled water, and dry for standby use;
[0008] S2: Apply a layer of molybdenum disulfide release agent on the inner wall of the mold, add the lower punch, foam copper, lead alloy, and upper punch into the mold in sequence, put the mold into a hot press furnace and heat it to 350°C, keep it warm for 20 minutes, and during the heat preservation process, apply pressure to the upper punch to make the molten lead liquid completely flow into the pores of the foam copper, wait for it to cool naturally to 80°C, and demold, to obtain a foam copper / lead alloy precursor;
[0009] S3: In sulfuric acid electrolyte, the foam copper / lead alloy precursor is used as the anode, the stainless steel plate is used as the cathode, and ammonium sulfate is used as the complexing agent. Constant current polarization is performed for 24 hours. When the anode potential is basically stable, the foam copper is completely dissolved to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure.
[0010] S4: 3D lead alloy is used as the matrix. The plating solution is prepared by 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles. The plating temperature is 60-80℃ and the current density is 0.015-0.025A / cm 2 , electroplating time 0.5 ~ 1.5h, mechanical stirring, adding PbO2-WC coating on the surface of 3D lead alloy;
[0011] S5: Sputtering of Co3O4 coating on 3D lead alloy substrate using RF magnetron sputtering.
[0012] Furthermore, the foam copper in S1 has a thickness of 6-8 mm, a pore diameter of 2-3 mm, and a porosity of 70-90%.
[0013] Furthermore, the WC particles in the S4 have a particle size of 1 to 3 μm, are soaked in 1:1 nitric acid for 1 to 3 hours before use, and then dispersed using ultrasound for 0.5 hours.
[0014] Furthermore, in S5, a Co3O4 (99.99%) disk with a diameter of 60 mm and a thickness of 3 mm is used as a sputtering target; in S5, the sputtering gas is argon with a purity of 99.999%.
[0015] Furthermore, before sputtering, the substrate is heated to 500°C and the sputtering chamber is first pumped down from atmospheric pressure to 1×10 3 Pa base pressure, the Co3O4 target was pre-sputtered in pure argon at 60W for 5min to remove the oxide layer or contaminants on the target surface. Under the condition of a total pressure of 1.0Pa, argon was introduced into the sputtering chamber at a gas flux of 4sccm. The substrate was fixed on the anode, and the distance between the target and the substrate was 120mm.
[0016] Furthermore, during the sputtering process of S5, the sputtering power of the Co3O4 target was fixed at 100 W, and the pure oxide phase (Co3O4) was obtained only by single-target sputtering. All the films were deposited within half an hour and cooled to room temperature in a high vacuum atmosphere.
[0017] Another object of the present invention is to provide a system for preparing a 3D porous structure lead alloy composite anode for implementing the method for preparing the 3D porous structure lead alloy composite anode, the system comprising:
[0018] Pretreatment module: Cut the lead alloy plate and the foam copper plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and foam copper in a prepared mixed sodium salt solution (20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, 20g / L sodium phosphate), soak for 3 minutes to remove oil stains on the surface of the foam aluminum, rinse with distilled water, and dry for standby use;
[0019] The foam copper / lead alloy precursor preparation module is connected to the pretreatment module, a layer of molybdenum disulfide release agent is applied on the inner wall of the mold, a lower punch, foam copper, lead alloy, and upper punch are sequentially added to the mold, the mold is placed in a hot press furnace and heated to 350°C, and the heat is kept for 20 minutes. During the heat preservation process, pressure is applied to the upper punch to make the molten lead liquid completely flow into the pores of the foam copper, and it is naturally cooled to 80°C, and then demolded to obtain a foam copper / lead alloy precursor;
[0020] The 3D lead alloy matrix preparation module is connected to the foam copper / lead alloy precursor preparation module. In sulfuric acid electrolyte, the foam copper / lead alloy precursor is used as an anode, a stainless steel plate is used as a cathode, and ammonium sulfate is used as a complexing agent. Constant current polarization is performed for 24 hours. When the anode potential is basically stable, the foam copper is completely dissolved to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure.
[0021] The plating module is connected to the 3D lead alloy substrate preparation module. The 3D lead alloy is used as the substrate. The plating solution is prepared by 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles. The plating temperature is 60-80℃, and the current density is 0.015-0.025A / cm 2 , electroplating time 0.5 ~ 1.5h, mechanical stirring, adding PbO2-WC coating on the surface of 3D lead alloy;
[0022] The sputtering module is connected to the coating module and uses a radio frequency magnetron sputtering method to sputter a Co3O4 coating on a 3D lead alloy substrate.
[0023] Another object of the present invention is to provide a 3D porous structure lead alloy composite anode system, the system comprising:
[0024] A cutting module, used to cut the lead alloy plate and the foam copper plate into shapes that meet the size of the mold;
[0025] A pretreatment module is used to soak the cut lead alloy and foam copper in a prepared mixed sodium salt solution to remove oil stains on the surface of the foam copper, and then rinse with distilled water and dry;
[0026] A hot pressing and melt infiltration module, used to combine the treated lead alloy and foam copper into a foam copper / lead alloy precursor through hot pressing and melt infiltration processes;
[0027] An electrochemical dissolution module is used to dissolve the copper foam by an electrochemical method to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure;
[0028] Electroplating module for electroplating PbO2-WC coating on 3D lead alloy substrate;
[0029] Sputtering module for sputtering Co3O4 coatings on 3D lead alloy substrates by RF magnetron sputtering.
[0030] Furthermore, the pretreatment module also includes an oil removal unit, which uses a mixed sodium salt solution containing sodium hydroxide, sodium silicate, sodium carbonate and sodium phosphate to effectively remove oil from the surface of the foam copper.
[0031] Furthermore, the electroplating module includes a plating solution preparation unit and an electroplating control unit. The plating solution preparation unit is used to prepare a plating solution containing lead nitrate, copper nitrate, sodium fluoride and WC particles. The electroplating control unit is used to control the temperature, current density and electroplating time during the electroplating process to form a uniform PbO2-WC coating on the surface of the 3D lead alloy.
[0032] Furthermore, the sputtering module includes a target material pretreatment unit, a sputtering control unit and a cooling unit. The target material pretreatment unit is used to pre-sputter the Co3O4 target material to remove the oxide layer or contaminants on the surface. The sputtering control unit is used to control the gas flux, sputtering power and sputtering time during the sputtering process to form a dense Co3O4 coating on the 3D lead alloy substrate. The cooling unit is used to cool the deposited film to room temperature in a high vacuum atmosphere.
[0033] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0034] First, the present invention effectively solves the problem of reduced service life of porous anodes, so WC and Co3O4 coatings are applied on the surface of 3D lead alloy to improve the corrosion resistance of the anode and further increase the electrochemical performance of the anode.
[0035] The present invention aims to provide a 3D porous structure lead alloy composite anode material, aiming to provide a new anode material with excellent electrochemical properties and corrosion resistance. The present invention aims to provide a preparation method of a 3D porous structure lead alloy composite anode material, aiming to prepare the special composite anode material.
[0036] Second, the expected benefits and commercial value of the technical solution of the present invention after transformation are: due to the porous structure, the contact between the anode and the electrolyte is greatly increased, the real current density of the anode is reduced, and the overpotential of the oxygen evolution reaction is reduced. The doping of Co3O4 and WC can not only reduce the overpotential of oxygen evolution, but also improve the corrosion resistance of the anode. Therefore, the research on the porous lead alloy-based PbO2-WC / Co3O4 composite anode has far-reaching scientific significance and economic benefits in the electrodeposition industry.
[0037] The technical solution of the present invention solves the technical problems that people have been eager to solve but have never succeeded in solving: the present invention adopts foam copper plate to prepare porous lead alloy, which overcomes the problem that some filler particles are covered by lead alloy liquid and cannot be removed in the infiltration casting method; the doping of WC and Co3O4 overcomes the problem of low life of porous anode.
[0038] Third, the preparation method of the 3D porous structure lead alloy composite anode provided by the present invention solves a series of technical problems of the traditional method in electrochemical applications. First, in the preparation process, the foam copper is treated by using a specific mixed sodium salt solution to effectively remove the surface oil stains, thereby ensuring the smooth progress of the subsequent process. Secondly, the combination of lead alloy and foam copper is precisely controlled by using molybdenum disulfide release agent and hot pressing process, ensuring the structural stability and electrochemical performance of the composite anode. Then, the composite anode is subjected to constant current polarization treatment in the electrolyte to achieve the comprehensive dissolution of the foam copper and form a 3D lead alloy matrix with a three-dimensional through-hole structure, thereby significantly improving the electrochemical activity and stability of the anode. Finally, in the plating and sputtering process, the preparation of PbO2-WC and Co3O4 composite coatings on the 3D lead alloy matrix is successfully achieved through precise parameter control and specific pre-treatment steps, providing a new functional material solution for electrochemical applications. These technological advances have given the composite anode a wider application prospect and more superior performance in the fields of batteries, electrolytic cells, etc.
[0039] Fourth, the present invention mainly relates to a method for preparing a 3D porous structure lead alloy composite anode, which specifically includes the following steps and parameters:
[0040] 1. Material preparation and degreasing (S1): Cut the lead alloy plate and the foam copper plate into shapes that meet the mold size using a wire cutting machine, soak them in the prepared mixed sodium salt solution for 3 minutes to remove the oil stains on the surface of the foam aluminum, then rinse them with distilled water and dry them. The foam copper has a thickness of 6-8 mm, a pore size of 2-3 mm, and a porosity of 70-90%.
[0041] 2. Hot pressing (S2): Apply a layer of molybdenum disulfide release agent on the inner wall of the mold, add the lower punch, foam copper, lead alloy and upper punch into the mold in sequence, heat to 350°C and keep warm for 20 minutes. Apply pressure during the insulation process to make the molten lead liquid completely flow into the pores of the foam copper, and demold after cooling to 80°C to obtain a foam copper / lead alloy precursor.
[0042] 3. Electrolytic dissolution (S3): In sulfuric acid electrolyte, with the foam copper / lead alloy precursor as the anode and the stainless steel plate as the cathode, constant current polarization is performed for 24 hours, and the foam copper is completely dissolved to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure.
[0043] 4. Electroplating PbO2-WC coating (S4): 3D lead alloy is used as the matrix in the plating solution, the plating temperature is 60-80℃, and the current density is 0.015-0.025A / cm 2The electroplating time is 0.5-1.5 hours, and the PbO2-WC coating is added to the surface of the 3D lead alloy by mechanical stirring. The WC particles have a particle size of 1-3μm and are soaked in 1:1 nitric acid for 1-3 hours before use, and then dispersed by ultrasonic for 0.5 hours.
[0044] 5. Sputtered Co3O4 coating (S5): A Co3O4 coating was sputtered on the 3D lead alloy substrate using a radio frequency magnetron sputtering method, using a Co3O4 (99.99%) disk with a diameter of 60 mm and a thickness of 3 mm.
[0045] Existing lead alloy anodes have problems such as unstable electrochemical performance, poor corrosion resistance and insufficient active surface area during use. These defects seriously affect the application effect and service life of lead alloy anodes, and it is difficult to meet the needs of high-performance electrolysis and electroplating. At the same time, the traditional preparation process is complicated and costly, making it difficult to promote and apply on a large scale. The present invention significantly improves the performance of lead alloy anodes by introducing 3D porous structure and composite coating design, and solves the key problems in the prior art.
[0046] The present invention prepares a 3D lead alloy matrix with a three-dimensional through-hole structure through hot pressing and electrolytic dissolution processes, increases the active surface area of the anode, and significantly improves the efficiency of the electrochemical reaction. At the same time, by electroplating a PbO2-WC coating and sputtering a Co3O4 coating on the surface of the 3D lead alloy matrix, the corrosion resistance and electrochemical stability of the anode are further enhanced. Mechanical stirring and ultrasonic dispersion technology are used to ensure the uniform distribution of WC particles in the plating solution, thereby improving the uniformity and quality of the coating.
[0047] The present invention introduces a scientific mathematical model and optimization algorithm in the preparation process, accurately controls various process parameters, and ensures the stability and repeatability of the preparation process. By optimizing material selection and process design, a 3D porous structure lead alloy composite anode with excellent performance is successfully prepared, showing excellent electrochemical properties and corrosion resistance. Practical applications show that the anode has a long service life and high electrochemical reaction activity in the electrolysis and electroplating process, significantly improves production efficiency, reduces maintenance costs, and has broad industrial application prospects and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a flow chart of a method for preparing a 3D porous structure lead alloy composite anode provided by an embodiment of the present invention;
[0049] Figure 2 It is a structural diagram of a preparation system of a 3D porous lead alloy composite anode provided in an embodiment of the present invention;
[0050] Figure 3Schematic diagram of a device for preparing a foam copper / lead alloy precursor provided in an embodiment of the present invention;
[0051] Figure 4 is a schematic diagram of the structure of a foam copper / lead alloy provided by an embodiment of the present invention;
[0052] Figure 5 It is a schematic diagram of the 3D lead alloy matrix provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0054] The following are two specific embodiments according to the preparation method provided:
[0055] Application Example 1:
[0056] 1. Material preparation and pretreatment:
[0057] The lead alloy plate and the foam copper plate are cut into shapes that match the size of the mold.
[0058] The cut lead alloy and foam copper are immersed in a mixed sodium salt solution for 3 minutes to remove the oil stains on the surface of the foam copper.
[0059] Rinse with distilled water and dry for later use. The foam copper has a thickness of 7 mm, a pore size of 2.5 mm, and a porosity of 80%.
[0060] 2. Hot pressing and melt penetration:
[0061] The inner wall of the mold is coated with molybdenum disulfide release agent.
[0062] Put the lower punch, foam copper, lead alloy and upper punch in sequence, and place them in a hot pressing furnace and heat them to 350°C for 20 minutes.
[0063] During the insulation process, pressure is applied to the upper punch to ensure that the molten lead liquid completely flows into the pores of the foam copper.
[0064] The mold was removed after naturally cooling to 80° C. to obtain a foamed copper / lead alloy precursor.
[0065] 3. Electrochemical dissolution and preparation of 3D lead alloy matrix:
[0066] In sulfuric acid electrolyte, with the precursor as the anode and the stainless steel plate as the cathode, constant current polarization was performed for 24 hours.
[0067] When the anode potential is stabilized, the copper foam is completely dissolved to form a 3D lead alloy matrix with a three-dimensional through-hole structure.
[0068] 4. Electroplating PbO2-WC coating:
[0069] The plating solution is prepared by 180 g / L lead nitrate, 15 g / L copper nitrate, 0.5 g / L sodium fluoride and 40 g / L WC particles (particle size 2 μm, soaked in nitric acid for 2 hours and ultrasonically dispersed for 0.5 hours).
[0070] At a temperature of 60 to 80°C, at 0.02A / cm 2 The electroplating was carried out at a current density of 1000 nm for 1 h with mechanical stirring during the electroplating.
[0071] 5. Sputtering Co3O4 coating:
[0072] Co3O4 was sputtered on a 3D lead alloy substrate heated to 500°C using RF magnetron sputtering.
[0073] Before sputtering, the pressure in the sputtering chamber was reduced to 1×10 3 Pa, pre-sputtered Co3O4 target at 60W for 5 minutes.
[0074] Argon gas was introduced at a gas flux of 4 sccm at a total pressure of 1.0 Pa, the target-substrate distance was 120 mm, and the sputtering power was 100 W.
[0075] The film was deposited for half an hour and cooled to room temperature in a high vacuum atmosphere.
[0076] Application Example 2:
[0077] This embodiment is substantially the same as Embodiment 1, but has the following differences:
[0078] 1. Material preparation: The thickness of the foam copper is 6mm, the pore diameter is 2mm, and the porosity is 70%.
[0079] 2. Electroplating PbO2-WC coating: the electroplating time is 0.5 hours.
[0080] 3. Sputtering Co3O4 coating: The sputtering time was 45 min to obtain Co3O4 coatings of different thicknesses.
[0081] These two examples demonstrate how to customize the performance of the 3D porous structure lead alloy composite anode by adjusting process parameters (such as electroplating time, foam copper specifications, sputtering time, etc.). Figure 1 As shown, a method for preparing a 3D porous structure lead alloy composite anode, the method comprising:
[0082] S1: Cut the lead alloy plate and the foam copper plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and foam copper in a prepared mixed sodium salt solution (20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, 20g / L sodium phosphate), soak for 3 minutes to remove oil stains on the surface of the foam aluminum, rinse with distilled water, and dry for standby use;
[0083] S2: Apply a layer of molybdenum disulfide release agent on the inner wall of the mold, add the lower punch, foam copper, lead alloy, and upper punch into the mold in sequence, put the mold into a hot press furnace and heat it to 350°C, keep it warm for 20 minutes, and during the heat preservation process, apply pressure to the upper punch to make the molten lead liquid completely flow into the pores of the foam copper, wait for it to cool naturally to 80°C, and demold, to obtain a foam copper / lead alloy precursor;
[0084] S3: In sulfuric acid electrolyte, the foam copper / lead alloy precursor is used as the anode, the stainless steel plate is used as the cathode, and ammonium sulfate is used as the complexing agent. Constant current polarization is performed for 24 hours. When the anode potential is basically stable, the foam copper is completely dissolved to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure.
[0085] S4: 3D lead alloy is used as the matrix. The plating solution is prepared by 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles. The plating temperature is 60-80℃ and the current density is 0.015-0.025A / cm 2 , electroplating time 0.5 ~ 1.5h, mechanical stirring, adding PbO2-WC coating on the surface of 3D lead alloy;
[0086] S5: Sputtering of Co3O4 coating on 3D lead alloy substrate using RF magnetron sputtering.
[0087] The foam copper in S1 has a thickness of 6-8 mm, a pore diameter of 2-3 mm, and a porosity of 70-90%.
[0088] The WC particles in the S4 have a particle size of 1 to 3 μm and are soaked in 1:1 nitric acid for 1 to 3 hours before use, and then dispersed by ultrasonic wave for 0.5 hours.
[0089] In the S5, a Co3O4 (99.99%) disk with a diameter of 60 mm and a thickness of 3 mm is used as a sputtering target; in the S5, the sputtering gas is argon gas with a purity of 99.999%.
[0090] Before sputtering, the substrate was heated to 500 °C and the sputtering chamber was first pumped down from atmospheric pressure to 1 × 10 3Pa base pressure, the Co3O4 target was pre-sputtered in pure argon at 60W for 5min to remove the oxide layer or contaminants on the target surface. Under the condition of a total pressure of 1.0Pa, argon was introduced into the sputtering chamber at a gas flux of 4sccm. The substrate was fixed on the anode, and the distance between the target and the substrate was 120mm.
[0091] During the sputtering process of S5, the sputtering power of the Co3O4 target was fixed at 100 W, and the pure oxidation phase (Co3O4) was obtained only by single-target sputtering. All the films were deposited within half an hour and cooled to room temperature in a high vacuum atmosphere.
[0092] like Figure 2 As shown, an embodiment of the present invention provides a system for preparing a 3D porous structure lead alloy composite anode for implementing the preparation method of the 3D porous structure lead alloy composite anode, the system comprising:
[0093] Pretreatment module: Cut the lead alloy plate and the foam copper plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and foam copper in a prepared mixed sodium salt solution (20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, 20g / L sodium phosphate), soak for 3 minutes to remove oil stains on the surface of the foam aluminum, rinse with distilled water, and dry for standby use;
[0094] The foam copper / lead alloy precursor preparation module is connected to the pretreatment module, a layer of molybdenum disulfide release agent is applied on the inner wall of the mold, a lower punch, foam copper, lead alloy, and upper punch are sequentially added to the mold, the mold is placed in a hot press furnace and heated to 350°C, and the heat is kept for 20 minutes. During the heat preservation process, pressure is applied to the upper punch to make the molten lead liquid completely flow into the pores of the foam copper, and it is naturally cooled to 80°C, and then demolded to obtain a foam copper / lead alloy precursor;
[0095] The 3D lead alloy matrix preparation module is connected to the foam copper / lead alloy precursor preparation module. In sulfuric acid electrolyte, the foam copper / lead alloy precursor is used as an anode, a stainless steel plate is used as a cathode, and ammonium sulfate is used as a complexing agent. Constant current polarization is performed for 24 hours. When the anode potential is basically stable, the foam copper is completely dissolved to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure.
[0096] The plating module is connected to the 3D lead alloy substrate preparation module. The 3D lead alloy is used as the substrate. The plating solution is prepared by 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles. The plating temperature is 60-80℃, and the current density is 0.015-0.025A / cm 2 , electroplating time 0.5 ~ 1.5h, mechanical stirring, adding PbO2-WC coating on the surface of 3D lead alloy;
[0097] The sputtering module is connected to the coating module and uses a radio frequency magnetron sputtering method to sputter a Co3O4 coating on a 3D lead alloy substrate.
[0098] An embodiment of the present invention provides a computer device, which includes a memory and a processor, wherein the memory stores a computer program, and when the computer program is executed by the processor, the processor executes the steps of the method for preparing the 3D porous structure lead alloy composite anode.
[0099] An embodiment of the present invention provides a computer-readable storage medium storing a computer program. When the computer program is executed by a processor, the processor executes the steps of the method for preparing the 3D porous structure lead alloy composite anode.
[0100] An embodiment of the present invention provides an information data processing terminal, which is used to implement a preparation system for the 3D porous structure lead alloy composite anode.
[0101] Example 13D-Pb-Ag / PbO2-WC / Co3O4 composite anode
[0102] The preparation method thereof comprises the following steps:
[0103] Step 1: Cut the Pb-Ag alloy and 8mm thick copper foam plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and copper foam in a prepared mixed sodium salt solution (20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, 20g / L sodium phosphate), soak for 3 minutes to remove oil stains on the surface of the aluminum foam, rinse with distilled water, and dry for use.
[0104] Step 2: Apply a layer of molybdenum disulfide release agent on the inner wall of the mold, and add the lower punch, foam copper, Pb-Ag alloy, and upper punch into the mold in sequence. Place the mold in a hot press furnace and heat it to 350°C for 20 minutes. During the heat preservation process, apply pressure to the upper punch to allow the molten lead to flow completely into the pores of the foam copper. Allow it to cool naturally to 80°C, demold, and obtain the foam copper / Pb-Ag precursor.
[0105] Step 3: In sulfuric acid electrolyte, the copper foam / Pb-Ag body is used as the anode, the stainless steel plate is used as the cathode, and ammonium sulfate is used as the complexing agent, and constant current polarization is performed for 24 hours. When the anode potential is basically stable, the copper foam is completely dissolved to obtain a 3D-Pb-Ag alloy matrix with a three-dimensional through-hole structure.
[0106] Step 4: Use 3D-Pb-Ag as the matrix. The plating solution is made of 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles (particle size 1-3μm, soaked in 1:1 nitric acid for 1h before use, and then dispersed by ultrasonic for 0.5h). The plating temperature is 70℃ and the current density is 0.02A / cm 2 , electroplating time 1h, mechanical stirring. The plating of PbO2-WC coating on the surface of 3D-Pb-Ag alloy is completed.
[0107] Step 5: Sputtering Co3O4 coating on 3D lead alloy substrate using RF magnetron sputtering, using Co3O4 (99.99%) disk with a diameter of 60 mm and a thickness of 3 mm as the sputtering target. The sputtering gas is argon with a purity of 99.999%. Before sputtering, the substrate is heated to 500 ° C, and the sputtering chamber is first pumped down from atmospheric pressure to a base pressure of 1×103Pa. The Co3O4 target is pre-sputtered in pure argon at 60W for 5min to remove the oxide layer or contaminants on the target surface. Argon is introduced into the sputtering chamber at a gas flux of 4sccm under a total pressure of 1.0Pa. The substrate is fixed on the anode, and the distance between the target and the substrate is 120mm. The sputtering power of the Co3O4 target is fixed at 100W during the sputtering process. The pure oxide phase (Co3O4) is obtained only by single-target sputtering. All films are deposited within half an hour and cooled to room temperature in a high vacuum atmosphere.
[0108] Anode potential test conditions: 38°C water bath heating, three-electrode system, anode is the prepared 3D porous structure composite anode, cathode is platinum electrode, reference electrode is saturated potassium sulfate, electrolyte is 160g / L H2SO4, current density is 500A / m 2 .
[0109] Cell voltage test conditions: 40°C water bath heating, the anode is the prepared composite anode, the electrolyte is industrial zinc smelting electrolyte (55g / L ZnSO4, 160g / L H2SO4 aqueous solution), and the cathode is an aluminum plate.
[0110] The 3D-Pb-Ag / PbO2-WC / Co3O4 composite anode prepared in this example has higher corrosion resistance than the current Pb-0.75wt.% Ag alloy anode used in industrial zinc electrowinning. Under the premise of the same anode volume, the amount of metal Ag in the anode can be reduced by about 28%; and the anode potential is 1.30V, a decrease of 59mV; the cell voltage is 2.91V, a decrease of 90mV.
[0111] Example 23D-Pb-Ca-Sn / PbO2-WC / Co3O4 composite anode
[0112] Step 1: Cut the Pb-Ca-Sn alloy and 8mm thick copper foam plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and copper foam in a prepared mixed sodium salt solution (20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, 20g / L sodium phosphate), soak for 3 minutes to remove oil stains on the surface of the aluminum foam, rinse with distilled water, and dry for standby use.
[0113] Step 2: Apply a layer of molybdenum disulfide release agent on the inner wall of the mold, and add the lower punch, foam copper, Pb-Ca-Sn alloy, and upper punch into the mold in sequence. Place the mold in a hot press furnace and heat it to 350°C for 20 minutes. During the heat preservation process, apply pressure to the upper punch to allow the molten lead to flow completely into the pores of the foam copper. Allow it to cool naturally to 80°C, demold, and obtain the foam copper / Pb-Ca-Sn precursor.
[0114] Step 3: In sulfuric acid electrolyte, the copper foam / Pb-Ca-Sn body is used as the anode, the stainless steel plate is used as the cathode, and ammonium sulfate is used as the complexing agent, and constant current polarization is performed for 24 hours. When the anode potential is basically stable, the copper foam is completely dissolved to obtain a 3D-Pb-Ag alloy matrix with a three-dimensional through-hole structure.
[0115] Step 4: Use 3D-Pb-Ca-Sn as the matrix. The plating solution is made of 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles (particle size 1-3μm, soaked in 1:1 nitric acid for 1h before use, and then dispersed by ultrasonic for 0.5h). The plating temperature is 70℃ and the current density is 0.02A / cm 2 , electroplating time 1h, mechanical stirring. The plating of PbO2-WC coating on the surface of 3D-Pb-Ca-Sn alloy is completed.
[0116] Step 5: Sputter the Co3O4 coating on the 3D lead alloy substrate using RF magnetron sputtering, using a Co3O4 (99.99%) disk with a diameter of 60 mm and a thickness of 3 mm as the sputtering target. The sputtering gas is argon with a purity of 99.999%. Before sputtering, the substrate is heated to 500°C and the sputtering chamber is first pumped down from atmospheric pressure to 1×10 3 Pa base pressure. The Co3O4 target was pre-sputtered at 60W in pure argon for 5 minutes to remove the oxide layer or contaminants on the target surface. Argon was introduced into the sputtering chamber at a gas flux of 4sccm under a total pressure of 1.0Pa. The substrate was fixed on the anode, and the distance between the target and the substrate was 120mm. The sputtering power of the Co3O4 target was fixed at 100W during the sputtering process. Pure oxidation phase (Co3O4) was obtained only by single target sputtering. All films were deposited within half an hour and cooled to room temperature in a high vacuum atmosphere.
[0117] The 3D-Pb-Ca-Sn / PbO2-WC / Co3O4 composite anode prepared in this example has better electrochemical performance than the current lead-calcium-tin alloy anode used in industrial zinc electrowinning. The anode potential is 1.33V, which is 56mV lower; the cell voltage is 3.02V, which is 80mV lower.
[0118] Comparative Example 13D-Pb-Ag / PbO2-WC composite anode
[0119] Compared with Example 1, the only difference is that instead of sputtering the Co3O4 coating on the alloy surface by magnetron sputtering, PbO2-WC is co-deposited on the surface of the 3D lead-silver alloy.
[0120] The prepared anode was tested by the method of Example 1, and the anode potential was measured to be 1.35V and the cell voltage to be 3.06V.
[0121] Comparative Example 2 Pb-Ag / PbO2-WC / Co3O4 composite anode
[0122] Compared with Example 1, the only difference is that no porous treatment is performed, but WC and Co3O4 coatings are directly added to the surface of the lead-silver alloy. Other operations and parameters are the same as Example 1.
[0123] The prepared anode was tested by the method of Example 1. The anode potential was 1.34 V and the cell voltage was 3.03 V, both of which were higher than those of Example 1.
[0124] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a 3D porous structure lead alloy composite anode, characterized in that: The method includes: S1: Cut the lead alloy plate and the foam copper plate into shapes that meet the mold size using a wire cutting machine, place the cut lead-silver alloy and foam copper in a prepared mixed sodium salt solution, the mixed sodium salt solution consists of 20g / L sodium hydroxide, 4g / L sodium silicate, 10g / L sodium carbonate, and 20g / L sodium phosphate, soak for 3 minutes to remove oil stains on the surface of the foam aluminum, rinse with distilled water, and dry for standby use; S2: Apply a layer of molybdenum disulfide release agent on the inner wall of the mold, add the lower punch, foam copper, lead alloy, and upper punch into the mold in sequence, put the mold into a hot press furnace and heat it to 350°C, keep it warm for 20 minutes, and during the heat preservation process, apply pressure to the upper punch to make the molten lead liquid completely flow into the pores of the foam copper, wait for it to cool naturally to 80°C, and demold, to obtain a foam copper / lead alloy precursor; S3: In sulfuric acid electrolyte, the foam copper / lead alloy precursor is used as the anode, the stainless steel plate is used as the cathode, and ammonium sulfate is used as the complexing agent. Constant current polarization is performed for 24 hours. When the anode potential is basically stable, the foam copper is completely dissolved to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure. S4: 3D lead alloy is used as the matrix. The plating solution is made of 180g / L lead nitrate, 15g / L copper nitrate, 0.5g / L sodium fluoride, and 40g / L WC particles. The plating temperature is 60-80℃ and the current density is 0.015-0.025A / cm 2 , electroplating time 0.5 ~ 1.5h, mechanical stirring, adding PbO2-WC coating on the surface of 3D lead alloy; S5: Sputtering of Co3O4 coating on 3D lead alloy substrate using RF magnetron sputtering.
2. The method for preparing the 3D porous structure lead alloy composite anode according to claim 1, characterized in that: The foam copper in S1 has a thickness of 6-8 mm, a pore diameter of 2-3 mm, and a porosity of 70-90%.
3. The method for preparing the 3D porous structure lead alloy composite anode according to claim 1, characterized in that: The WC particles in the S4 have a particle size of 1 to 3 μm and are soaked in 1:1 nitric acid for 1 to 3 hours before use, and then dispersed by ultrasonic wave for 0.5 hours.
4. The method for preparing the 3D porous structure lead alloy composite anode according to claim 1, characterized in that: In the S5, a Co3O4 disk with a diameter of 60 mm and a thickness of 3 mm is used as a sputtering target; in the S5, the sputtering gas is argon gas with a purity of 99.999%.
5. The method for preparing the 3D porous structure lead alloy composite anode according to claim 1, characterized in that: Before sputtering, the substrate was heated to 500 °C and the sputtering chamber was first pumped down from atmospheric pressure to 1 × 10 3 Pa base pressure, the Co3O4 target was pre-sputtered at 60W for 5min in pure argon to remove the oxide layer or contaminants on the target surface. Under the condition of a total pressure of 1.0Pa, argon was introduced into the sputtering chamber at a gas flux of 4sccm. The substrate was fixed on the anode, and the distance between the target and the substrate was 120mm.
6. The method for preparing the 3D porous structure lead alloy composite anode according to claim 1, characterized in that: During the sputtering process of S5, the sputtering power of the Co3O4 target was fixed at 100 W, and the pure oxidation phase was obtained only by single-target sputtering. All the films were deposited within half an hour and cooled to room temperature in a high vacuum atmosphere.
7. A system for preparing a 3D porous structure lead alloy composite anode for implementing the method for preparing a 3D porous structure lead alloy composite anode as described in any one of claims 1 to 6, characterized in that: The system includes: A cutting module, used to cut the lead alloy plate and the foam copper plate into shapes that meet the size of the mold; A pretreatment module is used to soak the cut lead alloy and foam copper in a prepared mixed sodium salt solution to remove oil stains on the surface of the foam copper, and then rinse with distilled water and dry; A hot pressing and melt infiltration module, used to combine the treated lead alloy and foam copper into a foam copper / lead alloy precursor through hot pressing and melt infiltration processes; An electrochemical dissolution module is used to dissolve the copper foam by an electrochemical method to obtain a 3D lead alloy matrix with a three-dimensional through-hole structure; Electroplating module for electroplating PbO2-WC coating on 3D lead alloy substrate; Sputtering module for sputtering Co3O4 coatings on 3D lead alloy substrates by RF magnetron sputtering.
8. The 3D porous structure lead alloy composite anode system according to claim 7, characterized in that: The pretreatment module also includes an oil removal unit, which uses a mixed sodium salt solution containing sodium hydroxide, sodium silicate, sodium carbonate and sodium phosphate to effectively remove oil from the surface of the foam copper.
9. The 3D porous structure lead alloy composite anode system according to claim 7, characterized in that: The electroplating module includes a plating solution preparation unit and an electroplating control unit. The plating solution preparation unit is used to prepare a plating solution containing lead nitrate, copper nitrate, sodium fluoride and WC particles. The electroplating control unit is used to control the temperature, current density and electroplating time during the electroplating process to form a uniform PbO2-WC coating on the surface of the 3D lead alloy.
10. The 3D porous structure lead alloy composite anode system according to claim 7, characterized in that: The sputtering module includes a target material pretreatment unit, a sputtering control unit and a cooling unit. The target material pretreatment unit is used to pre-sputter the Co3O4 target material to remove the oxide layer or contaminants on the surface. The sputtering control unit is used to control the gas flux, sputtering power and sputtering time during the sputtering process to form a dense Co3O4 coating on the 3D lead alloy substrate. The cooling unit is used to cool the deposited film to room temperature in a high vacuum atmosphere.