Recycled material PET polyester automobile safety belt braid and preparation process thereof
By using regenerated PET yarns and modified graphene oxide treated PET fibers, combined with in-situ polymerization technology of dopamine, low-carbon and environmentally friendly PET polyester automotive seat belt webbing is prepared, solving the existing technology's high carbon emissions and performance deficiency The problem has achieved efficient carbon emission reduction and performance improvement.
Patent Information
- Application Number
- CN202411197135.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-19
AI Technical Summary
The carbon emissions are high during the production of automotive seat belt webbing. The production of existing PET polyester yarns has insufficient low carbon and environmental protection, and the webbing performance is difficult to guarantee.
The recycled material PET polyester automotive safety belt webbing is used. PET recycled yarn is used as warp and weft yarn, combined with modified graphene oxide and dopamine for spinning to improve the mechanical properties and antistatic properties of the webbing and reduce carbon emissions.
It significantly reduces the carbon emissions of PET polyester automotive seat belt webbing, maintains good physical and chemical properties, and improves the low-carbon environmental protection and anti-static properties of the webbing.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of webbings, and more specifically, to a recycled material PET polyester automobile safety belt webbing and a preparation process thereof. Background Art
[0002] Ribbon is a narrow or tubular fabric made of various yarns. Ribbon is widely used in luggage, clothing, and transportation industries, such as car seat belts, child seat belts, backpack belts, clothing decorative belts, and seat belts for subways and buses.
[0003] The material currently used for car seat belt webbing is PET polyester industrial filament, which has different specifications from 100D to 1500D. The current carbon emissions in the production of PET polyester yarn is 4.56kg of CO2 for every kg of yarn product produced. With the development of automobiles and public transportation, the demand for car seat belt webbing is increasing, which makes the industry's carbon emissions remain high and the industry's low-carbon and environmental protection performance is poor. Summary of the invention
[0004] In order to improve the low-carbon and environmental protection of webbing production while ensuring that the performance of the webbing is not reduced, the present application provides a recycled material PET polyester automobile seat belt webbing and a preparation process thereof.
[0005] In the first aspect, the present application provides a recycled material PET polyester automobile safety belt webbing, which adopts the following technical solution: A recycled material PET polyester automobile safety belt webbing comprises 80-85% warp yarns, 8-12% weft yarns, 2-5% side yarns, 2-3% gripping threads, and 1-2% locking threads. The warp yarns and weft yarns are both made of PET recycled yarns, and the side yarns, gripping threads and locking threads are made of PET braided yarns.
[0006] By adopting the above technical solution, PET recycled yarn is used as the main body of the safety belt webbing and the warp and weft yarn with the largest area. The weight of the PET recycled yarn accounts for more than 88% of the whole. The carbon emission in the production process of the PET recycled yarn is much lower than that of the PET woven yarn, so that the carbon emission in the production process of the recycled material PET polyester automobile safety belt webbing is much lower than that of the PET polyester automobile safety belt webbing woven with PET woven yarn. At the same time, the PET recycled yarn has good tensile properties and strength, so that the woven safety belt webbing has good strength. Its physical and chemical properties are not reduced compared with those of the PET polyester automobile safety belt webbing woven with PET woven yarn, and at the same time, the low-carbon and environmental protection in the production process of the automobile safety belt webbing is improved; Recycled PET is obtained through chemical recycling of waste PET. The structural properties of recycled PET are similar to those of virgin PET. It has good physical and chemical properties and meets spinning requirements. It can be used to prepare PET recycled yarn. The hydrophilic modifier can effectively improve the hydrophilicity of PET recycled yarn, thereby improving the antistatic properties of PET recycled yarn.
[0007] Preferably, the hydrophilic modifier is dopamine and modified graphene oxide in a mass ratio of (0.42-0.54):(2.8-3.6).
[0008] By adopting the above technical scheme, dopamine can be polymerized in situ, and dopamine has good viscosity and more active groups, so that dopamine can form a layer of polydopamine film on the surface of PET fiber, which can effectively improve the loading rate of modified graphene oxide. The modified graphene oxide can be blended with PET fiber to enhance the hydrophilicity and mechanical properties of PET fiber, and can also be loaded on the surface of PET fiber to improve the conductivity and antistatic properties of PET fiber.
[0009] Preferably, the preparation method of the modified graphene oxide comprises the following steps: placing the graphene oxide in a sodium hydroxide solution, stirring it magnetically for 1-1.2 hours, transferring it to a reaction kettle, reacting it at 120-130° C. for 12-13 hours, washing it with water, and drying it to obtain the modified graphene oxide.
[0010] By adopting the above technical solution, after the graphene oxide undergoes a sodium hydroxide hydrothermal reaction, the hydrophilic groups such as hydroxyl and carboxyl groups on the surface increase, and at the same time, the specific surface area of the graphene oxide increases, which can effectively improve the loading rate of the graphene oxide and the degree of bonding with the recycled PET.
[0011] In the second aspect, the present application provides a preparation process of a recycled material PET polyester automobile seat belt webbing, which adopts the following technical solution: A preparation process of recycled PET polyester automobile safety belt webbing, comprising the following steps: Preparation of recycled PET: After the waste PET is subjected to alcoholysis with ethylene glycol, the alcoholysis liquid is subjected to an ester exchange reaction with methanol to obtain dimethyl terephthalate, and dimethyl terephthalate is polymerized with ethylene glycol to obtain recycled PET; Preparation of PET regenerated yarn: a portion of modified graphene oxide is blended with recycled PET and then spun to obtain PET fiber; the PET fiber is treated with dopamine in-situ polymerization and then loaded with the remaining modified graphene oxide to obtain PET regenerated yarn; Ribbon weaving: Use PET recycled yarn as warp and weft yarn, PET braided yarn as edge yarn, grab yarn and lock yarn to weave into a ribbon.
[0012] By adopting the above technical scheme, after the waste PET is alcoholyzed with ethylene glycol, the main components of the alcoholysis liquid are monomers to pentamers of ethylene terephthalate. After the alcoholysis liquid is subjected to an ester exchange reaction with formaldehyde, dimethyl terephthalate is obtained. Dimethyl terephthalate can be purified by recrystallization to remove impurities and dyes, and then polymerized with ethylene glycol to obtain recycled PET. The PET fiber obtained by blending the recycled PET and modified graphene oxide has good mechanical properties and tensile properties, and the PET recycled yarn has good hydrophilicity and antistatic properties, so that the woven ribbon has good physical properties and antistatic properties.
[0013] Preferably, in the step of preparing the PET regenerated yarn, the modified graphene oxide blended with the recycled PET accounts for 19-32% of the total amount of the modified graphene oxide.
[0014] By adopting the above technical scheme, the blended modified graphene oxide is controlled so that the PET fiber obtained by blending and spinning has good mechanical properties. The modified graphene oxide can be evenly mixed with the recycled PET and is not easy to agglomerate. The remaining modified graphene oxide can be well loaded on the surface of the PET fiber, thereby improving the hydrophilicity and antistatic properties of the PET recycled yarn.
[0015] Preferably, the PET fiber is subjected to in-situ polymerization of dopamine and loading of modified graphene oxide, comprising the following steps: dissolving dopamine in Tris-HCl buffer, adjusting the pH of the solution to 8.5, immersing the PET fiber in the solution, standing at room temperature for 24 hours, taking out, drying, and obtaining the PET fiber treated with in-situ polymerization of dopamine, ultrasonically dispersing the modified graphene oxide in water to form a modified graphene oxide solution, immersing the PET fiber treated with in-situ polymerization of dopamine in the modified graphene oxide solution, immersing and drying multiple times, with a single immersion time of 30-35 minutes and a drying temperature of 55-65°C, repeating 3-4 times, and obtaining PET regenerated yarn.
[0016] By adopting the above technical solution, dopamine is in situ polymerized on the surface of the PET fiber by impregnation, so that a layer of polydopamine is formed on the surface of the PET fiber. The polydopamine has good viscosity and can effectively increase the loading rate of the modified graphene oxide on the surface of the PET fiber.
[0017] Preferably, before the PET fiber is treated with dopamine, it is further treated as follows: the PET fiber is immersed in a mixed enzyme solution, in which the concentration of cutinase is 0.26-0.28 mg / mL, the concentration of laccase is 0.78-0.81 mg / mL, the treatment temperature is 60-70°C, and the treatment time is 2-2.2 h.
[0018] By adopting the above technical scheme, the mixed enzyme formed by the mixture of cutinase and laccase can treat the surface of PET fiber. The surface of PET fiber is treated by enzymatic hydrolysis reaction, and the hydrophilic groups on the surface of PET fiber are increased, which is beneficial to the polymerization of dopamine.
[0019] In summary, this application has the following beneficial effects: 1. Since the present application adopts PET recycled yarn as the main body of the seat belt webbing and the warp and weft yarn with the largest area, the carbon emissions in the production process of the PET recycled yarn are much lower than those in the PET woven yarn, so that the carbon emissions in the production process of the recycled material PET polyester car seat belt webbing are much lower than those in the PET polyester car seat belt webbing woven with PET woven yarn. At the same time, the PET recycled yarn has good tensile properties and strength, so that the woven seat belt webbing has good strength, and its physical and chemical properties are not reduced compared with those of the PET polyester car seat belt webbing woven with PET woven yarn, and at the same time, the low-carbon and environmental protection of the car seat belt webbing production process is improved.
[0020] 2. In this application, the recycled PET is obtained by chemical recycling of waste PET. The structural properties of the recycled PET are similar to those of the original PET, and it has good physical and chemical properties. At the same time, it meets the spinning requirements and can be used to prepare PET recycled yarn. The hydrophilic modifier can effectively improve the hydrophilicity of the PET recycled yarn, thereby improving the antistatic properties of the PET recycled yarn.
[0021] 3. In the present application, after the waste PET is subjected to alcoholysis with ethylene glycol, the main components of the alcoholysis liquid are monomers to pentamers of ethylene terephthalate. After the alcoholysis liquid is subjected to an ester exchange reaction with formaldehyde, dimethyl terephthalate is obtained. Dimethyl terephthalate can be purified by recrystallization to remove impurities and dyes, and then polymerized with ethylene glycol to obtain recycled PET. The PET fiber obtained by blending the recycled PET and modified graphene oxide has good mechanical properties and tensile properties. The PET recycled yarn has good hydrophilicity and antistatic properties, so that the woven ribbon has good physical properties and antistatic properties. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments. Preparation Example 1-2 of Modified Graphene Oxide
[0023] Preparation Example 1 The preparation method of modified graphene oxide comprises the following steps: placing 0.3 g of graphene oxide in 100 mL of 10 wt% sodium hydroxide solution, stirring with magnetic force for 1 hour, transferring to a reactor, reacting at 120° C. for 13 hours, washing with water, and drying to obtain modified graphene oxide.
[0024] Preparation Example 2 The preparation method of modified graphene oxide includes the following steps: placing 0.5 g of graphene oxide in 120 mL of 13 wt % sodium hydroxide solution, magnetically stirring for 1.2 h, transferring to a reactor, reacting at 130° C. for 12 h, washing with water, and drying to obtain modified graphene oxide. Example
[0025] Example 1 A recycled PET polyester car seat belt webbing comprises 80% warp yarn, 12% weft yarn, 5% side yarn, 2% gripping thread and 1% locking thread, wherein the warp yarn and the weft yarn are both made of PET recycled yarn, the side yarn, the gripping thread and the locking thread are made of PET braided yarn, the PET recycled yarn comprises 40g recycled PET and 3.1g hydrophilic modifier, the hydrophilic modifier is dopamine and modified graphene oxide in a mass ratio of 0.42:2.8, and the modified graphene oxide is the modified graphene oxide prepared in Preparation Example 1.
[0026] The preparation process of the above-mentioned recycled material PET polyester automobile safety belt webbing comprises the following steps: Preparation of recycled PET: After the waste PET is crushed, the waste PET, ethylene glycol and zinc acetate are mixed in a mass ratio of 2:1:0.004, nitrogen is introduced for protection, and the mixture is reacted at 196°C for 2.5 hours to obtain an alcoholysis solution. The alcoholysis solution, methanol and sodium hydroxide are mixed in a mass ratio of 1:3:0.002, and the mixture is reacted at 65°C for 1.5 hours. After the reaction, the mixture is filtered, dried and purified to obtain dimethyl terephthalate. Dimethyl terephthalate, ethylene glycol and manganese acetate are mixed in a mass ratio of 1:2.5:0.002, and the mixture is reacted at 220°C for 2.5 hours. Antimony trioxide is added in an amount equal to that of manganese acetate, and the mixture is reacted at 270°C for 3 hours to obtain recycled PET. Preparation of PET regenerated yarn: 0.513g of modified graphene oxide and recycled PET were melt-blended and spun to obtain PET fibers, and then the PET fibers were treated: 0.4g of dopamine was dissolved in Tris-HCl buffer (0.05mol / L, pH=7), the dopamine concentration was 3g / L, the pH of the solution was adjusted to 8.5, the PET fibers were immersed in the solution, and after standing at room temperature for 24h, they were taken out and dried to obtain PET fibers treated with dopamine in situ polymerization, 2.187g of modified graphene oxide was ultrasonically dispersed in water to form a modified graphene oxide solution with a concentration of 15g / L, the PET fibers treated with dopamine in situ polymerization were immersed in the modified graphene oxide solution, and immersed and dried multiple times, the single immersion time was 30min, and the drying temperature was 55°C. After repeating 3 times, PET regenerated yarn was obtained; Ribbon weaving: Use PET recycled yarn as warp and weft yarn, PET braided yarn as edge yarn, grab yarn and lock yarn to weave into a ribbon.
[0027] Example 2 A recycled PET polyester car seat belt webbing comprises 85% warp yarn, 8% weft yarn, 2% side yarn, 3% gripping thread and 2% locking thread, wherein the warp yarn and the weft yarn are both made of PET recycled yarn, the side yarn, the gripping thread and the locking thread are made of PET braided yarn, the PET braided yarn is JH-PETKJ produced by Hebei Jinhong Chemical Co., Ltd., the PET recycled yarn comprises 50g recycled PET and 4.2g hydrophilic modifier, the hydrophilic modifier is dopamine and modified graphene oxide in a mass ratio of 0.54:3.6, and the modified graphene oxide is the modified graphene oxide prepared in Preparation Example 2.
[0028] The preparation process of the above-mentioned recycled material PET polyester automobile safety belt webbing comprises the following steps: Preparation of recycled PET: After the waste PET is crushed, the waste PET, ethylene glycol and zinc acetate are mixed in a mass ratio of 2:1:0.004, nitrogen is introduced for protection, and the mixture is reacted at 196°C for 2.5 hours to obtain an alcoholysis solution. The alcoholysis solution, methanol and sodium hydroxide are mixed in a mass ratio of 1:3:0.002, and the mixture is reacted at 65°C for 1.5 hours. After the reaction, the mixture is filtered, dried and purified to obtain dimethyl terephthalate. Dimethyl terephthalate, ethylene glycol and manganese acetate are mixed in a mass ratio of 1:2.5:0.002, and the mixture is reacted at 220°C for 2.5 hours. Antimony trioxide is added in an amount equal to that of manganese acetate, and the mixture is reacted at 270°C for 3 hours to obtain recycled PET. Preparation of PET regenerated yarn: 1.168g of modified graphene oxide and recycled PET were melt-blended and spun to obtain PET fiber, and the PET fiber was treated: 0.55g of dopamine was dissolved in Tris-HCl buffer (0.05mol / L, pH=7), the dopamine concentration was 3g / L, the pH of the solution was adjusted to 8.5, and the PET fiber was immersed in the solution, and after standing at room temperature for 24h, it was taken out and dried to obtain PET fiber treated with dopamine in situ polymerization, 2.482g of modified graphene oxide was ultrasonically dispersed in water to form a 15g / L modified graphene oxide solution, and the PET fiber treated with dopamine in situ polymerization was immersed in the modified graphene oxide solution, and was immersed and dried multiple times, with a single immersion time of 35min and a drying temperature of 65°C. After repeating 4 times, PET regenerated yarn was obtained; Ribbon weaving: Use PET recycled yarn as warp and weft yarn, PET braided yarn as edge yarn, grab yarn and lock yarn to weave into a ribbon.
[0029] Example 3 The difference between Example 3 and Example 1 is that the hydrophilic modifier is dopamine and modified graphene oxide in a mass ratio of 0.3:3.2.
[0030] Example 4 The difference between Example 4 and Example 1 is that the hydrophilic modifier is dopamine and modified graphene oxide in a mass ratio of 0.7:2.8.
[0031] Example 5 The difference between Example 5 and Example 1 is that, in the preparation step of the PET regenerated yarn, the modified graphene oxide blended with the recycled PET accounts for 10% of the total amount of the modified graphene oxide.
[0032] Example 6 The difference between Example 6 and Example 1 is that in the preparation step of the PET regenerated yarn, the modified graphene oxide blended with the recycled PET accounts for 45% of the total amount of the modified graphene oxide.
[0033] Example 7 The difference between Example 7 and Example 1 is that before the PET fiber is treated with dopamine, it is also treated as follows: the PET fiber is immersed in a mixed enzyme solution at a bath ratio of 10:1, in which the concentration of cutinase is 0.26 mg / mL, the concentration of laccase is 0.81 mg / mL, the treatment temperature is 70°C, and the treatment time is 2 h.
[0034] Example 8 The difference between Example 8 and Example 1 is that before the PET fiber is treated with dopamine, it is also treated as follows: the PET fiber is immersed in a mixed enzyme solution at a bath ratio of 10:1, in which the concentration of cutinase is 0.28 mg / mL, the concentration of laccase is 0.78 mg / mL, the treatment temperature is 60°C, and the treatment time is 2.2 h.
[0035] Example 9 The difference between Example 9 and Example 1 is that in the mixed enzyme solution, the concentration of cutinase is 0.15 mg / mL, and the concentration of laccase is 0.9 mg / mL.
[0036] Example 10 The difference between Example 10 and Example 1 is that in the mixed enzyme solution, the concentration of cutinase is 0.35 mg / mL, and the concentration of laccase is 0.5 mg / mL. Comparative Example
[0037] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the PET fiber is prepared by spinning recycled PET, and the recycled PET is not blended with modified graphene oxide.
[0038] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the PET fiber is not treated with in-situ polymerization of dopamine, and the PET fiber is immersed in a modified graphene oxide solution for loading of modified graphene oxide.
[0039] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the PET fiber is produced by spinning recycled PET, that is, PET recycled yarn.
[0040] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the amount of the hydrophilic modifier added is 2.5 g.
[0041] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that the amount of the hydrophilic modifier added is 6 g. Detection Methods
[0042] According to the raw materials and preparation processes of Examples 1-10 and Comparative Examples 1-5, a seat belt webbing with a width of 47 mm and a thickness of 1 mm was prepared, and the elongation, breaking strength and resistivity of the seat belt webbing were tested. The testing methods of elongation and breaking strength refer to "GB 14166-2013 Safety belts, restraint systems, child restraint systems and ISOFIX child restraint systems for motor vehicle occupants", and the resistivity was measured using a LFY-406 fabric surface resistivity tester, and the results are recorded in Table 1.
[0043] Table 1 Elongation, breaking strength and surface resistivity of seat belt webbing project Elongation / % Breaking strength / kN Specific resistance value / Ω Example 1 12.91 30.69 <![CDATA[1.41×10 7 ]]> Example 2 12.83 30.54 <![CDATA[1.39×10 7 ]]> Example 3 11.92 28.68 <![CDATA[2.21×10 7 ]]> Example 4 11.86 28.71 <![CDATA[2.28×10 7 ]]> Example 5 11.59 29.12 <![CDATA[2.42×10 7 ]]> Example 6 11.62 29.31 <![CDATA[2.31×10 7 ]]> Example 7 13.08 30.23 <![CDATA[1.01×10 7 ]]> Example 8 13.11 30.25 <![CDATA[1.03×10 7 ]]> Example 9 12.86 29.98 <![CDATA[1.29×10 7 ]]> Example 10 12.92 30.05 <![CDATA[1.31×10 7 ]]> Comparative Example 1 10.21 28.75 <![CDATA[2.98×10 7 ]]> Comparative Example 2 10.16 28.91 <![CDATA[7.68×10 7 ]]> Comparative Example 3 9.38 28.12 <![CDATA[1.21×10 8 ]]> Comparative Example 4 11.34 28.31 <![CDATA[2.92×10 7 ]]> Comparative Example 5 11.25 28.29 <![CDATA[2.89×10 7 ]]> According to Table 1, Examples 1-2 and Comparative Examples 1-3, it can be seen that the elongation and breaking strength of the seat belt webbing prepared in Example 1-2 are better than those in Comparative Examples 1-3, and the specific resistance value of Example 1-2 is lower than that of Comparative Examples 1-3, indicating that the seat belt webbing in Example 1-2 has better antistatic properties. The PET fiber in Example 1-2 is prepared by spinning after blending recycled PET and modified graphene oxide, and the recycled PET yarn is prepared after dopamine treatment and modified graphene oxide loading. The surface of the modified graphene oxide contains active groups such as hydroxyl and carboxyl groups. At the same time, the modified graphene oxide has good mechanical properties. After the recycled PET and the modified graphene oxide are blended, the mechanical strength of the recycled PET can be improved, so that the webbing has better elongation and breaking strength, and the modified graphene oxide can effectively improve the hydrophilicity of the PET fiber, thereby improving the antistatic property of the PET fiber, and then the seat belt webbing has good antistatic properties and is not easy to generate static electricity during use.
[0044] When preparing the PET fiber of Comparative Example 1, modified graphene oxide is not used to blend with recycled PET, and the PET fiber does not contain modified graphene oxide, so that the mechanical properties and strength of the PET fiber prepared in Comparative Example 1 are slightly lower than those in Example 1, thereby affecting the mechanical properties and strength of the seat belt webbing; the surface of the PET fiber of Comparative Example 2 is not loaded with modified graphene oxide, and the modified graphene oxide has good hydrophilicity and conductivity, and can enhance the hydrophilicity and antistatic properties of the PET fiber. Comparative Example 2 is not loaded with modified graphene oxide, so that the hydrophilicity and antistatic properties of the PET fiber of Comparative Example 2 are reduced, thereby affecting the hydrophilicity and antistatic properties of the seat belt webbing; the PET fiber of Comparative Example 3 is directly spun from recycled PET, and is not blended with modified graphene oxide or loaded with modified graphene oxide on the surface, so that the hydrophilicity, mechanical properties, and antistatic properties of the PET fiber are reduced, thereby affecting the mechanical properties, hydrophilicity, and antistatic properties of the seat belt webbing.
[0045] Compared with Example 1, the elongation and breaking strength of Comparative Example 4-5 are inferior to those of Example 1, the specific resistivity of Comparative Example 4-5 is higher than that of Example 1, and the antistatic performance of Comparative Example 4-5 is inferior to that of Example 1. Comparative Example 4-5 changes the amount of hydrophilic modifier added, indicating that the amount of hydrophilic modifier added affects the mechanical strength and antistatic performance of the webbing. The amount of hydrophilic modifier added directly affects the amount of modified graphene oxide blended with recycled PET, the thickness and morphology of the polydopamine film on the surface of PET fibers, and the loading amount of modified graphene oxide on the surface of PET fibers.
[0046] If the amount of modified graphene oxide blended with recycled PET is too small, the strength of the PET fiber will decrease. If the amount is too large, the modified graphene oxide will easily agglomerate, thereby reducing the performance of the PET fiber. If the amount of dopamine used is too small, the thickness of the polydopamine film on the surface of the PET fiber will decrease, and the adhesion of the polydopamine film will decrease, thereby affecting the loading amount of the modified graphene oxide. If the amount of dopamine used is too large, the thickness of the polydopamine film on the surface of the PET fiber will be uneven and the morphology will be poor, thereby affecting the loading amount of the modified graphene oxide. When the modified graphene oxide is loaded on the surface of the PET fiber, if the addition amount is too high or too low, it will also affect the final loading amount of the modified graphene oxide, causing the loading amount of the modified graphene oxide to decrease, thereby affecting the hydrophilicity, mechanical strength and antistatic properties of the PET fiber.
[0047] Compared with Example 1, the elongation and breaking strength of Example 3-4 are inferior to those of Example 1, the specific resistivity of Example 3-4 is higher than that of Example 1, and the antistatic performance of Example 3-4 is inferior to that of Example 1. Example 3-4 changes the mass ratio of dopamine to modified graphene oxide, indicating that the mass ratio of dopamine to modified graphene oxide affects the mechanical strength and antistatic performance of the webbing. Changing the mass ratio of dopamine to modified graphene oxide directly affects the amount of dopamine added and the amount of modified graphene oxide added during blending and loading, thereby affecting the mechanical properties and strength of the PET fiber, affecting the thickness, morphology and adhesion of the polydopamine film, and further affecting the loading amount of modified graphene oxide on the surface of the PET fiber, resulting in a decrease in the mechanical properties, strength and hydrophilicity of the PET fiber, and further decreasing the mechanical strength and antistatic performance of the seat belt webbing.
[0048] Compared with Example 1, the elongation and breaking strength of Example 5-6 are inferior to those of Example 1, the specific resistivity of Example 5-6 is higher than that of Example 1, and the antistatic performance of Example 5-6 is inferior to that of Example 1. Example 5-6 changes the proportion of modified graphene oxide blended with recycled PET in the total amount of modified graphene oxide, indicating that the proportion of modified graphene oxide added during blending has an effect on the mechanical strength and antistatic performance of the webbing. The proportion of modified graphene oxide added during blending affects the amount of modified graphene oxide added during blending, thereby affecting the mechanical properties and strength of the PET fiber, and at the same time affects the amount of modified graphene oxide loaded on the surface of the PET fiber, thereby affecting the hydrophilicity and antistatic performance of the PET fiber, and ultimately reducing the strength, hydrophilicity and antistatic performance of the seat belt webbing.
[0049] Compared with Example 1, the specific resistivity of Example 7-8 is lower than that of Example 1, and the antistatic performance of Example 7-8 is better than that of Example 1. In Example 7-8, the PET fiber is subjected to enzyme treatment before being treated with dopamine, which indicates that the enzyme treatment has some influence on the antistatic performance of the webbing. After the surface of the PET fiber is treated with the mixed enzyme formed by mixing cutinase and laccase, the surface of the PET fiber contains more active groups, which is beneficial to the polymerization of dopamine, thereby increasing the loading amount of modified graphene oxide on the surface of the PET fiber.
[0050] Compared with Example 7, the specific resistivity of Example 9-10 is higher than that of Example 7, and the antistatic performance of Example 9-10 is inferior to that of Example 7. When the PET fiber is subjected to enzyme treatment in Example 9-10, the concentrations of cutinase and laccase are changed, indicating that the concentrations of cutinase and laccase have an effect on the antistatic performance of the ribbon. When cutinase and laccase are used in combination, there is a synergistic effect between the two. Controlling the concentrations of cutinase and laccase can optimize the synergistic effect between the two, and the surface treatment effect on the PET fiber is better.
[0051] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A recycled material PET polyester automobile safety belt webbing, characterized by: The invention comprises the following mass ratios: 80-85% warp yarn, 8-12% weft yarn, 2-5% side yarn, 2-3% grabbing thread and 1-2% locking thread, wherein the warp yarn and weft yarn are both made of PET recycled yarn, the PET recycled yarn comprises 40-50 parts of recycled PET and 3.1-4.2 parts of hydrophilic modifier, and the side yarn, grabbing thread and locking thread are made of PET braided yarn.
2. The recycled PET polyester automobile safety belt webbing according to claim 1, characterized in that: The hydrophilic modifier is dopamine and modified graphene oxide in a mass ratio of (0.42-0.54):(2.8-3.6).
3. The recycled PET polyester automobile safety belt webbing according to claim 2, characterized in that: The preparation method of the modified graphene oxide comprises the following steps: placing the graphene oxide in a sodium hydroxide solution, stirring it with a magnetic force for 1-1.2 hours, transferring it to a reaction kettle, reacting it at 120-130° C. for 12-13 hours, washing it with water, and drying it to obtain the modified graphene oxide.
4. A process for preparing a recycled material PET polyester automobile safety belt webbing according to any one of claims 1-3, characterized in that: The following steps are involved: Preparation of recycled PET: After the waste PET is subjected to alcoholysis with ethylene glycol, the alcoholysis liquid is subjected to an ester exchange reaction with methanol to obtain dimethyl terephthalate, and dimethyl terephthalate is polymerized with ethylene glycol to obtain recycled PET; Preparation of PET regenerated yarn: a portion of modified graphene oxide is blended with recycled PET and then spun to obtain PET fiber; the PET fiber is treated with dopamine in-situ polymerization and then loaded with the remaining modified graphene oxide to obtain PET regenerated yarn; Ribbon weaving: Use PET recycled yarn as warp and weft yarn, PET braided yarn as edge yarn, grab yarn and lock yarn to weave into a ribbon.
5. The process for preparing a recycled material PET polyester automobile safety belt webbing according to claim 4, characterized in that: In the preparation step of the PET regenerated yarn, the modified graphene oxide blended with the recycled PET accounts for 19-32% of the total amount of the modified graphene oxide.
6. The process for preparing a recycled material PET polyester automobile safety belt webbing according to claim 4, characterized in that: The PET fiber is subjected to in-situ polymerization of dopamine and loading of modified graphene oxide, comprising the following steps: dissolving dopamine in a Tris-HCl buffer, adjusting the pH of the solution to 8.5, immersing the PET fiber in the solution, standing at room temperature for 24 hours, taking out, drying, obtaining the PET fiber treated with in-situ polymerization of dopamine, ultrasonically dispersing the modified graphene oxide in water to form a modified graphene oxide solution, immersing the PET fiber treated with in-situ polymerization of dopamine in the modified graphene oxide solution, immersing and drying for multiple times, wherein the single immersion time is 30-35 minutes and the drying temperature is 55-65° C., and after repeating 3-4 times, a PET regenerated yarn is obtained.
7. The process for preparing a recycled material PET polyester automobile safety belt webbing according to claim 6, characterized in that: Before the PET fiber is treated with dopamine, it is further treated as follows: the PET fiber is immersed in a mixed enzyme solution, in which the concentration of cutinase is 0.26-0.28 mg / mL, the concentration of laccase is 0.78-0.81 mg / mL, the treatment temperature is 60-70°C, and the treatment time is 2-2.2 hours.
Citation Information
Patent Citations
Surface modified aramid fiber and preparation method thereof
CN105603717A
Graphene anti-ultraviolet regenerated fiber and preparation method thereof
CN113897699A
Method for preparing PET slice from waste PET material and product
CN114437322A
Method for preparing moisture-absorption antistatic polyester filament yarns from regenerated polyester fibers
CN116005448A
KR20220003409A