Preparation method of aluminum-based inorganic flexible passive daytime radiation cooling material

Aluminum-based inorganic flexible passive daytime radiation cooling materials were prepared by electrospinning technology, which solved the problems of easy aging of organic materials and high energy consumption of traditional refrigeration technology, and achieved efficient and environmentally friendly daytime radiation cooling effect.

CN118979340AActive Publication Date: 2024-11-19QINGDAO UNIV

Patent Information

Application Number
CN202411084297.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The organic components in existing passive daytime radiation cooling materials are prone to aging, leading to secondary environmental pollution. Furthermore, traditional refrigeration technologies are energy-intensive and have a net heating effect on the atmosphere. There is a lack of economical and durable inorganic cooling materials.

Method used

Aluminum-based inorganic flexible passive daytime radiation cooling material was prepared using electrospinning technology. Flexible inorganic nanofiber membranes were prepared by electrospinning, vacuum drying and high-temperature calcination to achieve multi-level sunlight scattering and reduce heat absorption and light emission.

Benefits of technology

The prepared aluminum-based inorganic flexible passive daytime radiation cooling material has excellent resistance to ultraviolet aging, high temperature resistance, and flexibility, achieving efficient passive daytime radiation cooling with significant cooling effect, and is environmentally friendly and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979340A_ABST
    Figure CN118979340A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an aluminum-based inorganic flexible passive daytime radiation cooling material. The preparation method comprises the following steps: S1, preparing a precursor solution; s2, the precursor solution is subjected to electrostatic spinning, and an aluminum-based flexible electrostatic spinning fiber membrane is prepared and collected; and S3, the aluminum-based flexible electrostatic spinning fiber membrane is dried through a vacuum drying oven, the dried aluminum-based flexible electrostatic spinning fiber membrane is placed in a muffle furnace to be subjected to high-temperature calcination, organic matter components are removed, and the aluminum-based inorganic flexible passive daytime radiation cooling material is obtained. According to the preparation method of the aluminum-based inorganic flexible passive daytime radiation cooling material, a flexible inorganic nanofiber membrane structure is prepared on the basis of an electrostatic spinning technology, multi-stage sunlight scattering can be achieved, and therefore heat absorption and light emission are reduced, and the aluminum-based inorganic flexible passive daytime radiation cooling material can be further used for effective passive daytime radiation cooling, and the service life of the aluminum-based inorganic flexible passive daytime radiation cooling material is prolonged. In addition to excellent daytime refrigeration performance, the fiber membrane also has excellent ultraviolet aging resistance, high temperature resistance, flexibility and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of passive radiation cooling, and in particular relates to a method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material. Background Art

[0002] As global warming intensifies, hot summer days are becoming more and more common. Therefore, cooling has become more important to human life. Current mainstream cooling technologies such as air conditioning consume a large amount of electricity and will produce greenhouse gases (CO2) and ozone depleting gases (CCl2F). In addition, these cooling technologies only transfer heat to different places on the earth, and do not make the heat disappear in the atmosphere. Therefore, most cooling technologies have a net heating effect on the atmosphere.

[0003] Passive daytime radiative cooling can achieve passive cooling, based on the large temperature difference between the earth (~300K) and outer space (~3K), by transferring excess heat to the cold outer space through thermal radiation. The reason why this cooling system does not rely on external energy consumption is that the cooling between the earth's surface and outer space is achieved by emitting infrared thermal radiation. This new and green cooling technology has received a lot of attention and extensive research at home and abroad in recent years.

[0004] Although many materials have been proven to have good passive daytime radiation cooling performance, the vast majority of commonly used materials contain organic components. The high-molecular organic materials in passive daytime radiation cooling materials are prone to aging under the irradiation of sunlight, and thus are very likely to produce secondary environmental pollution, while inorganic fiber membranes have excellent properties in terms of resistance to ultraviolet aging, high temperature resistance, flexibility, and tensile strength. This shows that economical and durable inorganic cooling materials provide a sustainable solution to problems such as the greenhouse effect and energy progress. At the same time, compared with other technologies, electrospinning technology has many advantages such as simple manufacturing, high preparation efficiency, simple structural parameter control, cheap raw materials, and complete manufacturing technology. Therefore, the present invention proposes a method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material. The flexible inorganic nanofiber membrane structure prepared based on electrospinning technology can achieve multi-level sunlight scattering, thereby reducing heat absorption and luminescence, and can be used for effective passive daytime radiation cooling. In addition to excellent daytime cooling performance, the fiber membrane also has excellent resistance to ultraviolet aging, high temperature resistance, flexibility and other properties.

[0006] To achieve the above object, the present invention provides a method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material, comprising the following steps:

[0007] S1. preparing a precursor solution;

[0008] S11, dissolving the aluminum-based compound in a two-component solvent, and adding an acidic mixed solute in small amounts and multiple times;

[0009] S12, adding 5 wt % of polyvinyl pyrrolidone as a spinning aid, stirring evenly to obtain a precursor solution;

[0010] S2, electrospinning the precursor solution to prepare and collect an aluminum-based flexible electrospun fiber membrane;

[0011] S3. Dry the aluminum-based flexible electrospun fiber membrane using a vacuum drying oven, and place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components, thereby obtaining an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0012] Preferably, in step S11, the aluminum-based compound is composed of aluminum chloride hexahydrate and aluminum isopropoxide in a mass ratio of 0.8:2 to 1:2; the two-component solvent is composed of water and anhydrous ethanol in a mass ratio of 0.93:1 to 1:1; and the acidic mixed solute is composed of tartaric acid and glacial acetic acid in a mass ratio of 3.9:50 to 4:50.

[0013] Preferably, in step S12, stirring is performed uniformly at a temperature of 20° C. to 70° C.

[0014] Preferably, in step S2, the process conditions of electrospinning are specifically as follows: the spinning temperature is 20°C to 40°C, the spinning humidity is 10% to 50%, the spinning voltage is 15.5kV to 20kV, the propulsion rate of the spinning solution is 0.5ml / h to 1.2ml / h, the distance between the spinneret and the collector is 10cm to 20cm, and the rotation speed of the drum collector is 200rpm to 500rpm.

[0015] Preferably, in step S3, the temperature of the vacuum drying oven is 70° C. to 90° C., and the drying time is 12 h to 16 h.

[0016] Preferably, in step S3, the muffle furnace is used for high temperature calcination at 900°C to 1200°C at a heating rate of 1°C / min to 5°C / min.

[0017] Beneficial effects of the present invention:

[0018] (1) The aluminum-based inorganic flexible passive daytime radiation cooling material prepared by the present invention aims to prepare a flexible pure inorganic nanofiber membrane structure based on electrospinning technology. Compared with the common high-molecular organic materials that are easily aged and decomposed under long-term sunlight exposure, it can effectively extend the service life and reduce the environmental pollution of waste high-molecular materials, and has practical value.

[0019] (2) The preparation process of the present invention is simple and the structural parameters are easy to control, so that the process has the ability to be mass-produced.

[0020] (3) The aluminum-based inorganic flexible passive daytime radiation cooling material prepared by the present invention has high reflectivity and high emissivity. In addition to excellent daytime cooling performance, the cooling material also has excellent anti-ultraviolet aging, high temperature resistance, flexibility and other properties. It can be better assembled on the actual building surface and takes into account the thermal insulation and fire prevention functions.

[0021] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a SEM image of the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 1 of the method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material of the present invention;

[0023] Figure 2 This is a spectrum curve diagram of the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 1 of the method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material of the present invention;

[0024] Figure 3 This is a diagram showing the actual outdoor cooling effect of the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 1 of the method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material of the present invention;

[0025] Figure 4 The stress-strain curve of the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 1 of the preparation method of an aluminum-based inorganic flexible passive daytime radiation cooling material of the present invention before and after being irradiated with ultraviolet light for 72 hours;

[0026] Figure 5 This is a SEM image of the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Comparative Example 1 of the preparation method of an aluminum-based inorganic flexible passive daytime radiation cooling material of the present invention;

[0027] Figure 6 This is a SEM image of the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Comparative Example 2 of the preparation method of an aluminum-based inorganic flexible passive daytime radiation cooling material of the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0029] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0030] A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material comprises the following steps:

[0031] S1. Prepare a precursor solution.

[0032] S11. Dissolve the aluminum-based compound in a two-component solvent and add the acidic mixed solute in small amounts and multiple times.

[0033] The aluminum-based compound is composed of aluminum chloride hexahydrate and aluminum isopropoxide in a mass ratio of 0.8:2 to 1:2. The two-component solvent is composed of water and anhydrous ethanol in a mass ratio of 0.93:1 to 1:1. The acidic mixed solute is composed of tartaric acid and glacial acetic acid in a mass ratio of 3.9:50 to 4:50.

[0034] S12, adding 5 wt % of polyvinyl pyrrolidone as a spinning aid, and stirring evenly at a temperature of 20° C. to 70° C. to obtain a precursor solution.

[0035] S2. Electrospin the precursor solution to prepare and collect aluminum-based flexible electrospun fiber membrane.

[0036] The specific process conditions of electrospinning are as follows: spinning temperature of 20°C to 40°C, spinning humidity of 10% to 50%, spinning voltage of 15.5kV to 20kV, propulsion rate of spinning solution of 0.5ml / h to 1.2ml / h, distance between spinneret and collector of 10cm to 20cm, and rotation speed of drum collector of 200rpm to 500rpm.

[0037] S3. Dry the aluminum-based flexible electrospun fiber membrane in a vacuum drying oven. The temperature of the vacuum drying oven is 70° C. to 90° C., and the drying time is 12 h to 16 h.

[0038] The dried aluminum-based flexible electrospun fiber membrane is placed in a muffle furnace for high-temperature calcination to remove organic components. The muffle furnace is calcined at a high temperature of 900°C to 1200°C at a heating rate of 1°C / min to 5°C / min to obtain an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0039] Embodiment 1

[0040] A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material comprises the following steps:

[0041] S1. Dissolve 10 g of aluminum chloride hexahydrate and 20 g of aluminum isopropoxide in 60 g of a mixed solvent of water and anhydrous ethanol in a mass ratio of 1:1, add 1.2 g of tartaric acid and 15 g of glacial acetic acid in small amounts and several times, and finally add 5 wt % of polyvinyl pyrrolidone as a spinning aid, and stir evenly at 60° C. to obtain a precursor solution.

[0042] S2. Electrospin the precursor solution to prepare and collect aluminum-based flexible electrospun fiber membrane.

[0043] The specific process conditions of electrospinning are as follows: spinning temperature is 27°C, spinning humidity is 25%, spinning voltage is 19kV, spinning solution propulsion rate is 0.8ml / h, distance between spinneret and collector is 20cm, and rotation speed of drum collector is 300rpm.

[0044] S3. Dry the aluminum-based flexible electrospun fiber membrane in a vacuum drying oven at a temperature of 80°C for 14 hours. Place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components. The muffle furnace is calcined at a high temperature of 1100°C at a heating rate of 1°C / min to obtain an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0045] like Figure 1 As shown, the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 1 is composed of multiple layers of fiber stacking, and many nanopores are formed between the fibers. The fiber surface is flat and smooth, and the fiber diameter is distributed between 200nm and 1.1μm, which is equivalent to the wavelength of the reflected light, so that the aluminum-based inorganic flexible passive daytime radiation cooling material has a strong sunlight reflection ability, and the aluminum-based inorganic flexible passive daytime radiation cooling material shows a high solar reflectivity.

[0046] like Figure 2 As shown, the aluminum-based inorganic flexible passive daytime radiation cooling material exhibits strong reflective ability, especially in the sunlight band, with an average reflectivity of 96.94% in the 0.3μm to 2.5μm band, and an average emissivity of 92.85% in the atmospheric window band, especially in the 8μm to 13μm band.

[0047] like Figure 3 As shown, under exposure to sunlight, when the ambient temperature reaches 37°C, the flexible inorganic material can achieve a cooling effect of up to 5°C compared with the blank control group (common building materials).

[0048] like Figure 4 As shown, the maximum positive stress of the aluminum-based inorganic flexible passive daytime radiation cooling material is 0.59 MPa, and the mechanical properties do not change significantly after irradiation with ultraviolet light.

[0049] Embodiment 2

[0050] A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material comprises the following steps:

[0051] S1. Dissolve 10 g of aluminum chloride hexahydrate and 20 g of aluminum isopropoxide in 60 g of a mixed solvent of water and anhydrous ethanol in a mass ratio of 1:1, add 1.2 g of tartaric acid and 15 g of glacial acetic acid in small amounts and several times, and finally add 5 wt % of polyvinyl pyrrolidone as a spinning aid, and stir evenly at 60° C. to obtain a precursor solution.

[0052] S2. Electrospin the precursor solution to prepare and collect aluminum-based flexible electrospun fiber membrane.

[0053] The specific process conditions of electrospinning are as follows: spinning temperature of 27°C, spinning humidity of 25%, spinning voltage of 20 kV, propulsion rate of spinning solution of 0.8 ml / h, distance between spinneret and collector of 20 cm, and rotation speed of drum collector of 300 rpm.

[0054] S3. Dry the aluminum-based flexible electrospun fiber membrane in a vacuum drying oven at a temperature of 80°C for 14 hours. Place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components. The muffle furnace is calcined at a high temperature of 1100°C at a heating rate of 1°C / min to obtain an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0055] The aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 2 is composed of multiple layers of stacked fibers, and many nanopores are formed between the fibers. The fiber surface is flat and smooth, and the fiber diameter is distributed between 200nm and 900nm.

[0056] Actual outdoor cooling tests show that the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 2 can achieve a maximum cooling effect of 4.8°C compared with the blank control group (common building materials).

[0057] Embodiment 3

[0058] A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material comprises the following steps:

[0059] S1. Dissolve 10 g of aluminum chloride hexahydrate and 20 g of aluminum isopropoxide in 60 g of a mixed solvent of water and anhydrous ethanol in a mass ratio of 1:1, add 1.2 g of tartaric acid and 15 g of glacial acetic acid in small amounts and several times, and finally add 5 wt % of polyvinyl pyrrolidone as a spinning aid, and stir evenly at 60° C. to obtain a precursor solution.

[0060] S2. Electrospin the precursor solution to prepare and collect aluminum-based flexible electrospun fiber membrane.

[0061] The specific process conditions of electrospinning are as follows: spinning temperature is 27°C, spinning humidity is 25%, spinning voltage is 19kV, spinning solution propulsion rate is 0.8ml / h, distance between spinneret and collector is 20cm, and rotation speed of drum collector is 300rpm.

[0062] S3. Dry the aluminum-based flexible electrospun fiber membrane in a vacuum drying oven at a temperature of 80°C for 14 hours. Place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components. The muffle furnace is calcined at a high temperature of 1100°C at a heating rate of 3°C / min to obtain an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0063] The aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 3 is composed of multiple layers of stacked fibers, and many nanopores are formed between the fibers. The fiber surface is flat and smooth, and the fiber diameter is distributed between 200nm and 900nm.

[0064] Actual outdoor cooling tests show that the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Example 3 can achieve a maximum cooling effect of 4.7°C compared with the blank control group (common building materials).

[0065] Comparative Example 1

[0066] A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material comprises the following steps:

[0067] S1. Dissolve 10 g of aluminum chloride hexahydrate and 20 g of aluminum isopropoxide in 60 g of a mixed solvent of water and anhydrous ethanol in a mass ratio of 1:1, add 1.2 g of tartaric acid and 15 g of glacial acetic acid in small amounts and several times, and finally add 5 wt % of polyvinyl pyrrolidone as a spinning aid, and stir evenly at 60° C. to obtain a precursor solution.

[0068] S2. Electrospin the precursor solution to prepare and collect aluminum-based flexible electrospun fiber membrane.

[0069] The specific process conditions of electrospinning are as follows: spinning temperature is 27°C, spinning humidity is 25%, spinning voltage is 19kV, spinning solution propulsion rate is 1.5ml / h, distance between spinneret and collector is 20cm, and rotation speed of drum collector is 300rpm.

[0070] S3. Dry the aluminum-based flexible electrospun fiber membrane in a vacuum drying oven at a temperature of 80°C for 14 hours. Place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components. The muffle furnace is calcined at a high temperature of 1100°C at a heating rate of 1°C / min to obtain an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0071] like Figure 5 As shown in the figure, there are a large number of beads in the aluminum-based inorganic flexible passive daytime radiation cooling material. The fiber morphology is closely related to the injection speed of the polymer solution. For given electrospinning conditions, increasing the injection speed, although the movement speed of the jet in the high-voltage electric field does not change much, the amount of charge carried by the jet will increase due to the increase in the corresponding flow rate, which leads to the strengthening of the instability of the jet.

[0072] If the entangled molecular chains in the polymer solution cannot effectively overcome the external force to be stretched and oriented, it is easy to cause the jet to solidify into beads along the axial direction, especially when the amount of injected solution is greater than the amount of solution forming the jet, beads are more likely to form in the fiber film. This bead structure has an adverse effect on the mechanical properties of the fiber.

[0073] Actual outdoor cooling tests show that the aluminum-based inorganic flexible passive daytime radiation cooling material prepared in Comparative Example 1 can only achieve a cooling effect of 1.3°C compared with the blank control group (common building materials).

[0074] Comparative Example 2

[0075] A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material comprises the following steps:

[0076] S1. Dissolve 10 g of aluminum chloride hexahydrate and 20 g of aluminum isopropoxide in 60 g of a mixed solvent of water and anhydrous ethanol in a mass ratio of 1:1, add 1.2 g of tartaric acid and 15 g of glacial acetic acid in small amounts and several times, and finally add 5 wt % of polyvinyl pyrrolidone as a spinning aid, and stir evenly at 60° C. to obtain a precursor solution.

[0077] S2. Electrospin the precursor solution to prepare and collect aluminum-based flexible electrospun fiber membrane.

[0078] The specific process conditions of electrospinning are as follows: spinning temperature is 27°C, spinning humidity is 25%, spinning voltage is 19kV, spinning solution propulsion rate is 0.8ml / h, distance between spinneret and collector is 20cm, and rotation speed of drum collector is 300rpm.

[0079] S3. Dry the aluminum-based flexible electrospun fiber membrane in a vacuum drying oven at a temperature of 80°C for 14 hours. Place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components. The muffle furnace is calcined at a high temperature of 1300°C at a heating rate of 1°C / min to obtain an aluminum-based inorganic flexible passive daytime radiation cooling material.

[0080] like Figure 6 As shown in the figure, the fiber surface of the aluminum-based inorganic flexible passive daytime radiation cooling material becomes rough and there are a lot of fiber breakage phenomena. During the high-temperature calcination process, the fiber surface treatment agent will volatilize, and fiber defects such as protrusions and cracks on the fiber surface will gradually appear, causing the mechanical strength to gradually decrease.

[0081] The resulting inorganic fiber membrane has poor flexibility and cannot be fully tested in actual outdoor cooling tests.

[0082] Therefore, the present invention adopts the above-mentioned method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material. The flexible inorganic nanofiber membrane structure prepared based on the electrospinning technology can achieve multi-level sunlight scattering, thereby reducing heat absorption and luminescence, and can be used for effective passive daytime radiation cooling. In addition to its excellent daytime cooling performance, the fiber membrane also has excellent resistance to UV aging, high temperature resistance, flexibility and other properties.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material, characterized in that: The following steps are involved: S1. preparing a precursor solution; S11, dissolving the aluminum-based compound in a two-component solvent, and adding an acidic mixed solute in small amounts and multiple times; S12, adding 5 wt % of polyvinyl pyrrolidone as a spinning aid, stirring evenly to obtain a precursor solution; S2, electrospinning the precursor solution to prepare and collect an aluminum-based flexible electrospun fiber membrane; S3. Dry the aluminum-based flexible electrospun fiber membrane using a vacuum drying oven, and place the dried aluminum-based flexible electrospun fiber membrane in a muffle furnace for high-temperature calcination to remove organic components, thereby obtaining an aluminum-based inorganic flexible passive daytime radiation cooling material.

2. The method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material according to claim 1, characterized in that: In step S11, the aluminum-based compound is composed of aluminum chloride hexahydrate and aluminum isopropoxide in a mass ratio of 0.8:2 to 1:2; the two-component solvent is composed of water and anhydrous ethanol in a mass ratio of 0.93:1 to 1:1; and the acidic mixed solute is composed of tartaric acid and glacial acetic acid in a mass ratio of 3.9:50 to 4:

50.

3. The method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material according to claim 1, characterized in that: In step S12, the mixture is stirred uniformly at a temperature of 20°C to 70°C.

4. The method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material according to claim 1, characterized in that: In step S2, the process conditions of electrospinning are specifically as follows: the spinning temperature is 20°C to 40°C, the spinning humidity is 10% to 50%, the spinning voltage is 15.5kV to 20kV, the propulsion rate of the spinning solution is 0.5ml / h to 1.2ml / h, the distance between the spinneret and the collector is 10cm to 20cm, and the rotation speed of the drum collector is 200rpm to 500rpm.

5. The method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material according to claim 1, characterized in that: In step S3, the temperature of the vacuum drying oven is 70°C to 90°C, and the drying time is 12h to 16h.

6. The method for preparing an aluminum-based inorganic flexible passive daytime radiation cooling material according to claim 1, characterized in that: In step S3, the muffle furnace is calcined at a high temperature of 900°C to 1200°C at a heating rate of 1°C / min to 5°C / min.

Citation Information

Patent Citations

  • Flexible alumina ceramic fiber and preparation method thereof

    CN102167567A

  • Flexible gamma-Al2O3 fiber membrane and preparing method thereof

    CN102758310A

  • Inorganic fiber powder for radiation cooling and preparation method thereof

    CN113604905A

  • Aluminum oxide flexible fiber and preparation method thereof

    CN115262032A

  • Inorganic radiation refrigeration material as well as preparation method and application thereof

    CN118146765A

Cited By

  • Flame-retardant radiation refrigeration film with excellent durability and preparation method thereof

    CN119640498A