Modified carbon fiber, thermoplastic composite material and preparation method thereof
Modified carbon fibers were prepared by growing ZIF-8 and dopamine coatings in situ on the surface of carbon fibers, combining zinc nitrate hexachloride and cetyl trimethyl ammonium bromide, and composited with thermoplastic polypropylene, and the thermoplastic composite materials were solved. The problem of insufficient medium tensile strength and impact resistance improves the bending stiffness and tensile resistance of the material, and is suitable for high-strength applications.
Patent Information
- Application Number
- CN202411098538.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-19
AI Technical Summary
The tensile strength and impact resistance of carbon fibers in existing thermoplastic composite materials are insufficient, resulting in the mechanical properties that cannot meet the needs when used in a strong impact environment, and the uneven dispersion of carbon fibers in the material affects the overall performance.
Modified carbon fibers with multiple heterogeneous interfaces were prepared by growing ZIF-8 in situ on the surface of carbon fibers, combining dopamine coating with zinc nitrate hexahydrate and cetyl trimethylammonium bromide, and composited with thermoplastic polypropylene , increase the bonding strength and heterojunction of the material, and improve the tensile resistance of the material.
The bending stiffness and tensile resistance of thermoplastic composites have been significantly improved, making it possible to replace aluminum profiles in a variety of applications to meet the needs of high strength and high stiffness.
Smart Images

Figure CN118979388A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of thermoplastic plastics, and in particular to a modified carbon fiber, a thermoplastic composite material and a preparation method thereof. Background Art
[0002] With the rapid development of the plastics industry, the demand for thermoplastic composites is increasing due to their advantages of being recyclable and reusable, and their high resource utilization rate. This has also brought about a series of problems. In order to solve the problems of insufficient mechanical properties and poor impact toughness of carbon fiber, scholars have increased their research on carbon fiber surface modification. This is particularly urgent in the field of thermoplastic prepregs. How to control the activity of the surface of carbon fiber-based thermoplastic composites to enhance the tensile strength of carbon fiber and adapt it to a stronger impact-resistant environment is particularly important. Therefore, how to modify the preparation of carbon fiber thermoplastic composites and their processing tools to a greater extent has a broad research background and research value.
[0003] Thermoplastic composites are mainly composed of matrix modified carbon fiber and thermoplastic polypropylene. The matrix mainly plays a bonding and load-bearing role. The modified carbon fiber is the main filler, which mainly enhances the impact resistance and deformation resistance of thermoplastic composites. Due to its poor toughness. Compared with other matrices, the thermoplastic polypropylene matrix has good chemical stability, simple molding process, excellent processing performance and other characteristics, and can be widely used in aerospace, automobile manufacturing and other fields. However, while bringing great convenience, the service conditions of thermoplastic polypropylene products are often used in strong impact environments. The added carbon fiber is unevenly dispersed inside the thermoplastic composite material, making it impossible for the overall mechanical properties required for service, resulting in the impact resistance of subsequent thermoplastic composite products cannot be guaranteed, and the research and development and use are seriously affected. How to modify the surface activity of carbon fiber is the top priority of current research.
[0004] In the prior art, traditional additives are added to carbon fiber composite materials to increase the dispersion between fillers and thermoplastic matrix. However, considering the filler itself to enhance the impact resistance of thermoplastic composite materials is a new idea. How to modify the filler itself to enhance it to meet the needs of thermoplastic composite materials is the focus of current research by scientists. Summary of the invention
[0005] The main purpose of the present application is to propose a modified carbon fiber, a thermoplastic composite material and a preparation method thereof, aiming to provide a thermoplastic composite material with high bending stiffness.
[0006] To achieve the above-mentioned object, the first aspect of the present application proposes a modified carbon fiber, which comprises the following components by weight:
[0007]
[0008] The second aspect of the present application provides a method for preparing the modified carbon fiber of the first aspect, comprising:
[0009] Weigh carbon fiber, dopamine, dimethylimidazole, zinc nitrate hexahydrate, and hexadecyltrimethylammonium bromide respectively according to their mass fractions;
[0010] The carbon fibers were pretreated with acetone;
[0011] The pretreated carbon fiber is coated with dopamine so that dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer;
[0012] adding zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide to achieve in-situ growth of ZIF-8 on the surface of the carbon fiber coated with the polydopamine coating layer to obtain a mixture;
[0013] The mixture is washed and dried, and the dried powder is treated under an argon atmosphere to obtain modified carbon fibers.
[0014] In one embodiment, the carbon fiber is pretreated with acetone, comprising:
[0015] Adding carbon fiber into acetone, ultrasonically treating the carbon fiber for a first preset time and allowing the carbon fiber to stand for a second preset time to remove surface slurry;
[0016] The carbon fibers after surface slurry removal are centrifuged.
[0017] In one embodiment, the pretreated carbon fiber is coated with dopamine so that dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer, comprising:
[0018] Pour the pretreated carbon fiber into a container containing a preset mass fraction of deionized water;
[0019] Add dimethylimidazole to the container to adjust the pH value of the solution;
[0020] Dopamine is added to the container, and stirred for a third preset time using a magnetic stirrer under light-proof conditions, so that the dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer.
[0021] In one embodiment, zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide are added to achieve in-situ growth of ZIF-8 on the surface of a carbon fiber coated with a polydopamine coating layer, comprising:
[0022] Zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide are added to the carbon fiber solution coated with the polydopamine coating layer, and the magnetic stirrer is stirred for a fourth preset time to ensure that ZIF-8 is uniformly nucleated and grown on the surface of the carbon fiber coated with the polydopamine coating layer.
[0023] In one embodiment, the mixture is washed and dried, and the dried powder is treated under an argon atmosphere to obtain a modified carbon fiber, comprising:
[0024] The mixture was washed with deionized water and ethanol;
[0025] drying the washed mixture in a vacuum oven at a first preset temperature to obtain a powder;
[0026] The powder is heated to a second preset temperature at a preset heating rate under an argon atmosphere and then kept warm to obtain a modified carbon fiber.
[0027] The third aspect of the present application provides a thermoplastic composite material, which comprises the following components in parts by mass:
[0028]
[0029] In one embodiment, the toughening agent is a di-tetra-sulfurizer or a maleic anhydride grafted compatibilizer.
[0030] In one embodiment, the auxiliary agent is a diffusion oil.
[0031] A fourth aspect of the present application provides a method for preparing the thermoplastic composite material according to the third aspect, the method comprising:
[0032] Weigh the modified carbon fiber, thermoplastic polypropylene, toughening agent, and additives respectively according to their mass fractions;
[0033] The modified carbon fiber, thermoplastic polypropylene, toughening agent and auxiliary agent are added into a thermoplastic extruder for compression and melting to extrude the thermoplastic composite material.
[0034] Beneficial effects of this application:
[0035] The modified carbon fiber prepared by the present invention is modified on the basis of the original carbon fiber, and dopamine is polymerized in situ on the surface of the carbon fiber to provide conditions for the subsequent in situ growth of ZIF-8, and then zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide are added to achieve the in situ growth of ZIF-8 on the surface of the carbon fiber coated with a polydopamine coating layer, and a mixture is obtained. The obtained mixture is cleaned and dried to obtain a powder, and the powder is treated under an argon atmosphere to obtain a ZnNC / C@CF modified carbon fiber with multiple heterogeneous interfaces. The modified carbon fiber obtained by the modification is compounded with thermoplastic polypropylene, and the introduction of nitrogen-doped carbon nano-skeleton can well increase the combination with the thermoplastic resin, and the introduction of zinc element provides a richer heterojunction surface. Different chemical compositions and crystal structures in the heterogeneous interface will cause lattice strain, increase the adsorption energy of the site to the intermediate, increase grain boundary strengthening, and increase the tensile strength of the thermoplastic composite material to the outside world, so that the prepared thermoplastic composite material profile has higher bending stiffness and can replace aluminum profiles in many application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Schematic diagram of the process of preparing modified carbon fiber provided in the embodiment of the present application;
[0037] Figure 2 It is a schematic diagram of the process of preparing the thermoplastic composite material provided in the embodiment of the present application. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0039] It should be noted that although a logical order is shown in the flowchart, in some cases, the steps shown or described may be performed in a different order than that in the flowchart. The terms "first", "second", etc. in the specification, claims and the above drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.
[0041] The modified carbon fiber, thermoplastic composite material and preparation method thereof provided in the embodiments of the present application are specifically described through the following embodiments.
[0042] Example 1
[0043] A modified carbon fiber comprises the following components by mass: 20 wt% of carbon fiber, 3 wt% of dopamine, 47 wt% of dimethylimidazole, 20 wt% of zinc nitrate hexahydrate, and 10 wt% of hexadecyltrimethylammonium bromide.
[0044] like Figure 1 As shown, the preparation method of modified carbon fiber comprises:
[0045] S110, weighing raw materials according to the formula ratio.
[0046] S120, pretreating the carbon fiber with acetone, specifically:
[0047] The carbon fiber is added to acetone, and ultrasonically treated with an ultrasonic cleaner for a first preset time and allowed to stand for a second preset time to remove the surface slurry; the carbon fiber after the surface slurry is removed is centrifuged to separate the clean carbon fiber. It can be understood that the first preset time and the second preset time can be set according to actual needs. For example, the first preset time is 2 hours and the second preset time is 12 hours.
[0048] S130, coating the pretreated carbon fiber with dopamine so that dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer, specifically:
[0049] Pour the pretreated carbon fiber into a container containing a preset mass fraction of deionized water; add dimethylimidazole to the container to adjust the pH value of the solution; add dopamine to the container and stir with a magnetic stirrer for a third preset time under light-proof conditions to polymerize dopamine on the surface of the pretreated carbon fiber to form a polydopamine coating. It is understandable that the preset mass fraction and the third preset time can be set according to actual needs. For example, the preset mass fraction is 80wt% and the third preset time is 6h.
[0050] S140, adding zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide to achieve in-situ growth of ZIF-8 on the surface of the carbon fiber coated with the polydopamine coating layer, to obtain a mixture, specifically:
[0051] Zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide are added to the carbon fiber solution coated with the polydopamine coating layer, and the magnetic stirrer is stirred for a fourth preset time to ensure that ZIF-8 is uniformly nucleated and grown on the surface of the carbon fiber coated with the polydopamine coating layer. It can be understood that the fourth preset time can be set according to actual needs, and illustratively, the fourth preset time is 2 hours.
[0052] S150, washing and drying the mixture, and treating the dried powder under an argon atmosphere to obtain modified carbon fiber, specifically:
[0053] The mixture was washed several times with deionized water and ethanol; the washed mixture was dried in a vacuum oven at a first preset temperature to obtain a powder; the powder was heated to a second preset temperature at a preset heating rate under an argon atmosphere and then kept warm for 2 hours to obtain a modified carbon fiber with multiple heterogeneous interfaces of ZnNC / C@CF. It can be understood that the first preset temperature, the preset heating rate, and the second preset temperature can all be set according to actual needs. For example, the first preset temperature is 60°C, the preset heating rate is 3°C / min, and the second preset temperature is 600°C.
[0054] Example 2
[0055] A modified carbon fiber comprises the following components by mass: 10 wt% of carbon fiber; 5 wt% of dopamine; 52 wt% of dimethylimidazole; 25 wt% of zinc nitrate hexahydrate; and 8 wt% of hexadecyltrimethylammonium bromide.
[0056] The preparation method is the same as Example 1.
[0057] Example 3
[0058] A modified carbon fiber comprises the following components by mass: 30 wt% of carbon fiber; 1 wt% of dopamine; 42 wt% of dimethylimidazole; 15 wt% of zinc nitrate hexahydrate; and 12 wt% of hexadecyltrimethylammonium bromide.
[0059] The preparation method is the same as Example 1.
[0060] Example 4
[0061] A thermoplastic composite material comprises the following components in parts by mass: 10 wt % of the modified carbon fiber prepared in Example 1; 80 wt % of thermoplastic polypropylene; 4 wt % of a maleic anhydride grafted compatibilizer; and 6 wt % of a diffusion oil.
[0062] like Figure 2 As shown, a method for preparing a thermoplastic composite material comprises:
[0063] S210, weigh the raw materials according to the formula ratio.
[0064] S220, adding the raw materials into a thermoplastic extruder to compress and melt, and extruding a thermoplastic composite material.
[0065] It can be understood that the head shape of the thermoplastic extruder can be customized according to the profile requirements, such as I-beam type.
[0066] It can also be understood that the thermoplastic extruder can be heated to a predetermined temperature, illustratively, 180-300°C, and then the screw of the thermoplastic extruder is started, wherein the screw speed can be set according to different profiles. When the profile cross-section is large, the demand for resin is large, and the corresponding screw speed is fast, and vice versa; and raw materials are added, wherein the raw materials can be pre-mixed and added to the thermoplastic extruder, or can be mixed evenly in the thermoplastic extruder, and the mixed raw materials are compressed and melted in the screw of the thermoplastic extruder. After passing through the die mouth, the plastic is in a molten state and has a large plastic deformation ability, and deforms according to the shape of the die. After exiting the die, it enters the cooling and shaping stage. Most of this stage can be cooled with normal temperature water. High surface requirements can be adjusted to high temperature water to make the resin have some plasticity, so that the surface can be pressed smooth in combination with the pressure of the cooling roller. The cooling water is controlled by the mold temperature controller, and the water temperature can be adjusted to 0-100°C. The length of the cooling section can be set according to the wall thickness of the profile. If the wall thickness of the profile is very thick, it needs to be lengthened to achieve a sufficient cooling effect. Finally, the thermoplastic composite material continues to move under the continuous traction of the traction device, where the traction speed matches the screw speed, that is, the cross-sectional area of the profile (m 2 ) multiplied by the pulling speed (m / min) equals the extrusion volume (volume m 3 ). After traction, it is curled or cut according to actual needs.
[0067] Example 5
[0068] A thermoplastic composite material comprises the following components in parts by mass: 20 wt% of the modified carbon fiber prepared in Example 3; 70 wt% of thermoplastic polypropylene; 6 wt% of a di-tetra-sulfurizing agent; and 4 wt% of a diffusion oil.
[0069] The preparation method is the same as Example 4.
[0070] Example 6
[0071] A thermoplastic composite material comprises the following components in parts by mass: 30 wt% of the modified carbon fiber prepared in Example 2; 60 wt% of thermoplastic polypropylene; 8 wt% of a di-tetra-sulfurizing agent; and 2 wt% of a diffusion oil.
[0072] The preparation method is the same as Example 4.
[0073] The mechanical properties of the thermoplastic composite materials prepared in Examples 4-6 were measured using a universal testing machine. The results are shown in Table 1.
[0074] Comparative Example 1
[0075] A thermoplastic composite material is prepared by a method substantially the same as that of Example 5, except that no modified carbon fiber is added to the raw materials for preparing the thermoplastic composite material, but only pure carbon fiber is added.
[0076] Comparative Example 2
[0077] A thermoplastic composite material is prepared by a method substantially the same as that of Example 5, except that the raw material for synthesizing ZIF-8, i.e., zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide, is not added to the modified carbon fiber in the raw materials for preparing the thermoplastic composite material.
[0078] The mechanical properties of the thermoplastic composite materials prepared in Comparative Examples 1 and 2 were measured by a universal testing machine. The results are shown in Table 1.
[0079] Table 1 Mechanical properties
[0080] Tensile strength / MPa Compressive strength / MPa Bending strength / MPa Flexural modulus / GPa Example 4 90 54 120 5.3 Example 5 120 72 168 8.8 Example 6 115 62 140 6.7 Comparative Example 1 78 45 102 4.2 Comparative Example 2 82 47 106 4.6
[0081] By comparing Examples 4, 5, and 6, it can be seen that the mechanical properties of the thermoplastic composite material of Example 5 are the best. Therefore, it can be obtained that as the proportion of modified carbon fibers in the raw materials increases, the mechanical properties of the thermoplastic composite material will also increase. However, when it increases to a certain extent, if the proportion of modified carbon fibers continues to increase, the mechanical properties of the thermoplastic composite material will decrease instead.
[0082] By comparing Example 5 with Comparative Example 1, it can be found that, with the same proportion of raw materials, the mechanical properties of the thermoplastic composite material with the modified carbon fiber added are much greater than the mechanical properties of the thermoplastic composite material with the pure carbon fiber added.
[0083] By comparing Example 5 with Comparative Example 2, it can be obtained that, under the same proportion of raw materials, the mechanical properties of the thermoplastic composite material with modified carbon fiber added are much greater than the mechanical properties of the thermoplastic composite material with carbon fiber only coated with dopamine without adding zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide. It can be proved that the introduction of heterogeneous interfaces can increase the lattice strain caused by compression caused by different chemical components and crystal structures in the heterogeneous structure, increase the adsorption energy of the site to the intermediate, increase the grain boundary strengthening, and increase the compressive resistance of the thermoplastic composite material to the outside world, which fully meets the current era's demand for thermoplastic composite materials to cope with high impact and pressure-resistant environments, and has a more far-reaching impact on the future development of thermoplastic composite materials.
[0084] The present invention composites the modified carbon fiber with thermoplastic polypropylene to obtain a thermoplastic composite material with excellent impact resistance.
[0085] The implementation methods described in the embodiments of the present application are intended to more clearly illustrate the technical solutions of the embodiments of the present application, and do not constitute a limitation on the technical solutions provided in the embodiments of the present application. Those skilled in the art will appreciate that with the evolution of technology and the emergence of new application scenarios, the technical solutions provided in the embodiments of the present application are also applicable to similar technical problems.
[0086] The various embodiments in the present application are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0087] It should also be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, commodity, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity, or apparatus.
[0088] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A modified carbon fiber, characterized in that: The modified carbon fiber comprises the following components in parts by mass:
2. A method for preparing modified carbon fiber according to claim 1, characterized in that: include: Weigh carbon fiber, dopamine, dimethylimidazole, zinc nitrate hexahydrate, and hexadecyltrimethylammonium bromide respectively according to their mass fractions; Pretreating the carbon fiber with acetone; The pretreated carbon fiber is coated with dopamine so that dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer; adding zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide to achieve in-situ growth of ZIF-8 on the surface of the carbon fiber coated with the polydopamine coating layer to obtain a mixture; The mixture is washed and dried, and the powder obtained by drying is treated under an argon atmosphere to obtain the modified carbon fiber.
3. The method for preparing modified carbon fiber according to claim 2, characterized in that: The carbon fiber is pretreated with acetone, comprising: Adding the carbon fiber into the acetone, ultrasonically treating the carbon fiber for a first preset time and allowing the carbon fiber to stand for a second preset time to remove surface slurry; The carbon fibers after surface slurry removal are centrifuged.
4. The method for preparing modified carbon fiber according to claim 2, characterized in that: The method of coating the pretreated carbon fiber with dopamine so that dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer comprises: Pour the pretreated carbon fiber into a container containing a preset mass fraction of deionized water; Add dimethylimidazole to the container to adjust the pH value of the solution; Dopamine is added to the container, and stirred for a third preset time using a magnetic stirrer under light-proof conditions, so that the dopamine is polymerized on the surface of the pretreated carbon fiber to form a polydopamine coating layer.
5. The method for preparing modified carbon fiber according to claim 2, characterized in that: The method of adding zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide to achieve in-situ growth of ZIF-8 on the surface of the carbon fiber coated with the polydopamine coating layer comprises: The zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide are added to the carbon fiber solution coated with the polydopamine coating layer, and the magnetic stirrer is stirred for a fourth preset time to ensure that ZIF-8 is uniformly nucleated and grown on the surface of the carbon fiber coated with the polydopamine coating layer.
6. The method for preparing modified carbon fiber according to claim 2, characterized in that: The mixture is cleaned and dried, and the powder obtained by drying is treated under an argon atmosphere to obtain the modified carbon fiber, comprising: washing the mixture with deionized water and ethanol; drying the washed mixture in a vacuum oven at a first preset temperature to obtain a powder; The powder is heated to a second preset temperature at a preset heating rate under an argon atmosphere and then kept warm to obtain the modified carbon fiber.
7. A thermoplastic composite material, characterized in that: The thermoplastic composite material comprises the following components in parts by mass:
8. The thermoplastic composite material according to claim 7, characterized in that: The toughening agent is a di-tetra-sulfurizing agent or a maleic anhydride grafted compatibilizer.
9. The thermoplastic composite material according to claim 7, characterized in that: The auxiliary agent is diffusion oil.
10. A method for preparing a thermoplastic composite material according to any one of claims 7 to 9, characterized in that: The method comprises: Weigh the modified carbon fiber, thermoplastic polypropylene, toughening agent, and additives respectively according to their mass fractions; The modified carbon fiber, thermoplastic polypropylene, toughening agent and auxiliary agent are added into a thermoplastic extruder for compression and melting to extrude a thermoplastic composite material.