Waterproof moisture-permeable fabric and production process thereof

By covalent bonding of modified sodium alginate and modified emulsion to form a modified coating agent, combined with hydrogen bonds and fabric fibers, the polyethylene oxide side chain and hydrophobic properties are used to solve the insufficient waterproof and moisture-permeable fabric waterproof performance. The problem of this achieves efficient waterproof and moisture-permeable effect and mechanical performance improvement.

CN118979392APending Publication Date: 2024-11-19ANHUI JUCHUANG CHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411051118.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing waterproof and moisture-permeable fabrics are difficult to improve the waterproof performance of the fabric while retaining the breathable performance of the polyoxyethylene chain segment, resulting in a weakening of the mechanical properties of the fabric.

Method used

Modified sodium alginate and isocyanate groups in the modified emulsion are covalently bonded to form a modified coating agent, and hydrogen bonded with fabric fibers through the modification coating agent to form a dense polyurethane coating, using poly The ethylene oxide side chain realizes the permeation of gaseous water molecules, and at the same time, the hydrophobic properties of modified sodium alginate are used to improve the waterproofing properties.

Benefits of technology

The waterproof and mechanical properties of the fabric are improved, while maintaining the moisture permeability effect. Through the density and hydrophobicity of the modified coating agent, the effective permeability of gaseous water molecules is achieved, and the waterproof and moisture permeability of the fabric is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974957890000071
    Figure BDA0004974957890000071
  • Figure BDA0004974957890000081
    Figure BDA0004974957890000081
Patent Text Reader

Abstract

The invention discloses a waterproof and moisture permeable fabric and a production process thereof, and belongs to the technical field of textile fabrics, the production process comprises the following steps: S1, adding modified sodium alginate into a modified emulsion, stirring and mixing to obtain a modified coating agent; and S2, carrying out water repellent treatment, one-time dipping and one-time rolling on a polyester fabric, drying, uniformly coating the modified coating agent, and drying to obtain the waterproof and moisture permeable fabric. The modified emulsion is used as a base material of the modified coating agent, the modified sodium alginate with hydrophobic performance is used as a thickening agent, the modified emulsion and the modified sodium alginate are associated through a covalent bond, the mechanical property of the fabric coating is improved, meanwhile, a waterborne polyurethane main chain in the modified coating agent can form a compact polyurethane coating on the surface of the fabric, and the surface of the fabric can be effectively improved. According to the waterproof fabric provided by the invention, external water molecules are effectively prevented from permeating, the waterproof performance of the fabric is improved, the hydrophilic polyoxyethylene side chain can provide a path for vaporous water molecules to permeate for the compact coating, and the good moisture permeability of the fabric is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile fabrics, and in particular relates to a waterproof and breathable fabric and a production process thereof. Background Art

[0002] With the continuous improvement of technology and people's quality of life, waterproof and breathable fabrics are becoming more and more popular. Waterproof and breathable fabrics are functional fabrics that can block external moisture while allowing the sweat produced by the human body to be discharged in the form of water vapor. They are also called "breathable fabrics."

[0003] In the prior art, when processing textiles, water-based polyurethane with a polyethylene oxide structure in the main chain is usually used as a coating for the fabric. The polyethylene oxide segment has excellent hydrophilic properties and can provide a hydrophilic channel for the fabric to achieve a breathable and moisture-permeable effect. However, the direct introduction of the polyethylene oxide segment will not only reduce the waterproof effect of the coated fabric, but also reduce the film-forming properties of the water-based polyurethane, resulting in a weakening of the mechanical properties of the fabric, limiting the application of water-based polyurethane in waterproof and moisture-permeable surfaces. Therefore, how to improve the waterproof performance of the fabric while retaining the breathability of the polyethylene oxide segment is a technical problem that needs to be solved at present. Summary of the invention

[0004] The object of the present invention is to provide a waterproof and breathable fabric and a production process thereof to solve the problems in the background technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A production process of a waterproof and breathable fabric comprises the following steps:

[0007] S1, adding modified sodium alginate to the modified emulsion, stirring and mixing, to obtain a modified coating agent; using the modified sodium alginate as a thickener, and covalently bonding the amino group in the modified sodium alginate with the isocyanate group in the modified emulsion to obtain a modified coating agent in which the two are associated;

[0008] S2. The polyester fabric is subjected to water repellent treatment, dipped and rolled, and after drying, the modified coating agent is evenly coated, and then dried to obtain a waterproof and breathable fabric.

[0009] Furthermore, the weight ratio of the modified emulsion to the modified sodium alginate is 90-100:0.5-3.

[0010] Furthermore, the coating thickness is 80-100 μm.

[0011] Further, the modified emulsion is prepared by the following steps:

[0012] A1. Add 2,3-dihydroxysuccinic acid and polyethylene glycol monomethyl ether to toluene, stir to dissolve, add p-toluenesulfonic acid, reflux at 130-140° C. for 22-24 hours, add excess anhydrous sodium bicarbonate, stir and mix for 30 minutes, filter, and then perform rotary evaporation on the filtrate to obtain a modified polyether ester; use p-toluenesulfonic acid as a catalyst, 2,3-dihydroxysuccinic acid and polyethylene glycol monomethyl ether as reaction monomers, and use excess anhydrous sodium bicarbonate to neutralize unreacted 2,3-dihydroxysuccinic acid and p-toluenesulfonic acid to obtain a modified polyether ester containing hydroxyl groups and polyethylene oxide segments.

[0013] A2. Under nitrogen protection, add poly(1,4-butylene adipate) diol to acetone, stir and mix, add modified polyether ester and isophorone diisocyanate, stir and mix, then drop stannous octoate, stir and react at 80-90°C for 3-4h, cool to 45-50°C, add trimethylolpropane, react at 70-75°C for 2-3h, cool to 20-25°C, and post-treat to obtain a modified emulsion; stannous octoate is used as a catalyst, trimethylolpropane is used as a chain extender, poly(1,4-butylene adipate) diol and isophorone diisocyanate are used as raw materials, and combined with the hydroxyl group in the modified polyether ester, a modified emulsion with a waterborne polyurethane as the main chain and a polyethylene oxide segment as the side chain is obtained.

[0014] Furthermore, the usage ratio of toluene, 2,3-dihydroxysuccinic acid, polyethylene glycol monomethyl ether and p-toluenesulfonic acid is 100 mL: 6-10 g: 15-21 mL: 0.5 g.

[0015] Furthermore, the usage ratio of the acetone, poly(1,4-butylene adipate diol), modified polyether ester, isophorone diisocyanate, stannous octoate and trimethylolpropane is 80 mL: 14-21 g: 2-3 mL: 7-9 mL: 0.2 mL: 0.4-0.8 g.

[0016] Furthermore, the post-treatment is to add 200 mL of deionized water, emulsify for 20-30 minutes, then dropwise add 2 mL of 0.3-0.5 wt% ethylenediamine aqueous solution as a post-chain extender, stir for 10 minutes, and then perform rotary evaporation.

[0017] Furthermore, the modified sodium alginate is prepared by the following steps:

[0018] Add sodium alginate to a phosphate buffer solution, stir to dissolve, add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stir to mix, then add N-hydroxysuccinimide, stir to mix, then add octylamine, stir to react at 20-25° C. for 22-24 hours, then place in anhydrous ethanol for alcohol precipitation, centrifuge, wash, and dry to obtain modified sodium alginate; use 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride as a catalyst and N-hydroxysuccinimide as an activating agent, graft the long alkyl chain segment of octylamine to the molecule of sodium alginate through an amidation reaction to obtain modified sodium alginate with hydrophobic properties.

[0019] Furthermore, the dosage ratio of the phosphate buffer solution, sodium alginate, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and octylamine is 100mL: 2-4g: 0.5-1g: 0.3-0.9g: 0.8-1mL; and the pH value of the phosphate buffer solution is 5-6.

[0020] A waterproof and breathable fabric is made by the above production process.

[0021] Beneficial effects of the present invention:

[0022] The modified coating agent of the present invention contains hydroxyl groups on its molecular chain, which can be combined with fabric fibers through hydrogen bonds, thereby improving the interface bonding force between the modified coating agent and the fabric. At the same time, the water-based polyurethane main chain in the modified coating agent can form a dense polyurethane coating on the surface of the fabric, effectively preventing external water molecules from penetrating, thereby improving the waterproof performance of the fabric. The hydrophilic polyethylene oxide side chain can provide a path for gaseous water molecules to penetrate the dense coating. When the human body produces sweat and evaporates, the gaseous water molecules will be adsorbed on the polyethylene oxide segment in the coating, diffuse outward under the action of the temperature and humidity difference between the inside and outside of the coated fabric, transfer the gaseous water molecules on the inside to the outside, and desorb under the action of the hydrophobic octane segment introduced by the modified sodium alginate, so as to achieve the effect of moisture permeability and breathability, thereby giving the fabric excellent waterproof and moisture permeability.

[0023] The present invention uses a modified latex as a base material of a modified coating agent, uses modified sodium alginate with hydrophobic properties as a thickener, and combines the isocyanate group in the modified latex with the amide group of the modified sodium alginate through a covalent bond, which is beneficial to improving the film-forming property of the modified coating agent and enhancing the mechanical properties of the fabric coating, and can also improve the density of the fabric coating and further improve the waterproof property of the fabric. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] This embodiment provides a modified emulsion, which is prepared by the following steps:

[0027] A1. Add 6 g of 2,3-dihydroxysuccinic acid and 15 mL of polyethylene glycol monomethyl ether to 100 mL of toluene, stir to dissolve, add 0.5 g of p-toluenesulfonic acid, reflux at 130 ° C for 22 h, add excess anhydrous sodium bicarbonate, stir and mix for 30 min, filter, and then rotary evaporate the filtrate to obtain modified polyether ester;

[0028] A2. Under nitrogen protection, add 14 g of poly(1,4-butylene adipate) diol to 80 mL of acetone, stir and mix, add 2 mL of modified polyether ester and 7 mL of isophorone diisocyanate, stir and mix, then drop 0.2 mL of stannous octoate, stir and react at 80 ° C for 3 h, cool to 45 ° C, add 0.4 g of trimethylolpropane, react at 70 ° C for 2 h, cool to 20 ° C, add 200 mL of deionized water, emulsify for 20 min, then drop 2 mL of 0.3 wt% ethylenediamine aqueous solution, stir for 10 min, and then perform rotary evaporation to obtain a modified emulsion.

[0029] Example 2

[0030] This embodiment provides a modified emulsion, which is prepared by the following steps:

[0031] A1. Add 8 g of 2,3-dihydroxysuccinic acid and 17 mL of polyethylene glycol monomethyl ether to 100 mL of toluene, stir to dissolve, add 0.5 g of p-toluenesulfonic acid, reflux at 135 ° C for 23 h, add excess anhydrous sodium bicarbonate, stir and mix for 30 min, filter, and then rotary evaporate the filtrate to obtain a modified polyether ester;

[0032] A2. Under nitrogen protection, add 18g of poly(1,4-butylene adipate)diol to 80mL of acetone, stir and mix, add 2.5mL of modified polyether ester and 8mL of isophorone diisocyanate, stir and mix, then drop 0.2mL of stannous octoate, stir and react at 85°C for 3.5h, cool to 48°C, add 0.6g of trimethylolpropane, react at 73°C for 2.5h, cool to 22°C, add 200mL of deionized water, emulsify for 25min, drop 2mL of 0.4wt% ethylenediamine aqueous solution, stir for 10min, and then perform rotary evaporation to obtain a modified emulsion.

[0033] Example 3

[0034] This embodiment provides a modified emulsion, which is prepared by the following steps:

[0035] A1. Add 10 g of 2,3-dihydroxysuccinic acid and 21 mL of polyethylene glycol monomethyl ether to 100 mL of toluene, stir to dissolve, add 0.5 g of p-toluenesulfonic acid, reflux at 140 °C for 24 h, add excess anhydrous sodium bicarbonate, stir and mix for 30 min, filter, and then rotary evaporate the filtrate to obtain a modified polyether ester;

[0036] A2. Under nitrogen protection, add 21g of poly(1,4-butylene adipate)diol to 80mL of acetone, stir and mix, add 3mL of modified polyether ester and 9mL of isophorone diisocyanate, stir and mix, then drop 0.2mL of stannous octoate, stir and react at 90°C for 4h, cool to 50°C, add 0.8g of trimethylolpropane, react at 75°C for 3h, cool to 25°C, add 200mL of deionized water, emulsify for 30min, drop 2mL of 0.5wt% ethylenediamine aqueous solution, stir for 10min, and then perform rotary evaporation to obtain a modified emulsion.

[0037] Example 4

[0038] This embodiment provides a modified sodium alginate, which is prepared by the following steps:

[0039] Add 2 g of sodium alginate to 100 mL of phosphate buffer solution with a pH value of 5, stir to dissolve, add 0.5 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stir to mix, then add 0.3 g of N-hydroxysuccinimide, stir to mix, then add 0.8 mL of octylamine, stir to react at 20° C. for 22 hours, then place in anhydrous ethanol for alcohol precipitation, centrifuge, wash, and dry to obtain modified sodium alginate.

[0040] Example 5

[0041] This embodiment provides a modified sodium alginate, which is prepared by the following steps:

[0042] To 100 mL of phosphate buffer solution with a pH value of 5.5, 3 g of sodium alginate was added and stirred to dissolve, 0.7 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride was added and stirred to mix, and then 0.6 g of N-hydroxysuccinimide was added and stirred to mix, and then 0.9 mL of octylamine was added and stirred to react at 22° C. for 23 h, and then placed in anhydrous ethanol for alcohol precipitation, and after centrifugation, washing and drying, modified sodium alginate was obtained.

[0043] Example 6

[0044] This embodiment provides a modified sodium alginate, which is prepared by the following steps:

[0045] To 100 mL of phosphate buffer solution with a pH value of 6, 4 g of sodium alginate was added, and the mixture was stirred to dissolve. 1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride was added, and the mixture was stirred to mix. Then, 0.9 g of N-hydroxysuccinimide was added, and the mixture was stirred to mix. Then, 1 mL of octylamine was added, and the mixture was stirred to react at 25° C. for 24 h. The mixture was then placed in anhydrous ethanol for precipitation. After centrifugation, washing, and drying, modified sodium alginate was obtained.

[0046] Example 7

[0047] This embodiment provides a production process for a waterproof and breathable fabric, comprising the following steps:

[0048] S1. Add 0.5 parts by weight of modified sodium alginate to 90 parts by weight of the modified latex, stir and mix to obtain a modified coating agent;

[0049] S2. The polyester fabric is treated with water repellent, dipped and rolled, and after drying, the modified coating agent is evenly coated with a coating thickness of 80 μm, and then dried to obtain a waterproof and breathable fabric.

[0050] Example 8

[0051] This embodiment provides a production process for a waterproof and breathable fabric, comprising the following steps:

[0052] S1. Add 2 parts by weight of modified sodium alginate to 95 parts by weight of the modified latex, stir and mix to obtain a modified coating agent;

[0053] S2. The polyester fabric is treated with water repellent, dipped and rolled, and after drying, the modified coating agent is evenly coated with a coating thickness of 90 μm, and then dried to obtain a waterproof and breathable fabric.

[0054] Example 9

[0055] This embodiment provides a production process for a waterproof and breathable fabric, comprising the following steps:

[0056] S1. Add 3 parts by weight of modified sodium alginate to 100 parts by weight of the modified latex, stir and mix, and obtain a modified coating agent;

[0057] S2. The polyester fabric is treated with water repellent, dipped and rolled, and after drying, the modified coating agent is evenly coated with a coating thickness of 100 μm, and then dried to obtain a waterproof and breathable fabric.

[0058] Comparative Example 1: Compared with Example 7, the modified coating agent was replaced with an equal amount of an organosilicon coating agent, and the rest was the same.

[0059] Comparative Example 2: Compared with Example 7, modified sodium alginate was not added, and the rest was the same.

[0060] Comparative Example 3: Compared with Example 7, the modified latex was replaced by an equal amount of an aqueous polyurethane having a polyethylene oxide segment introduced into the main chain, and the rest was the same.

[0061] Performance tests were performed on Examples 7 to 9 and Comparative Examples 1 to 3. Waterproof performance test: the samples were made into 15 cm × 15 cm specimens, and the test was performed using a water permeability tester in accordance with GB / T 4744-2013, and the hydrostatic pressure value when the third water droplet emerged was recorded; Moisture permeability test: the moisture permeability test was performed in accordance with GB / T12704-1991; Mechanical performance test: the modified coating agent was evenly coated on a polytetrafluoroethylene plate, and the tensile strength of the coating film was tested in accordance with GB / T 19250-2013. The results are shown in Table 1:

[0062] Table 1

[0063]

[0064]

[0065] It can be seen from Table 1 that the hydrostatic pressure value and moisture permeability of the fabrics prepared by the modified coating agent in Examples 7-9 are significantly greater than those in Comparative Examples 1-3, and have good waterproof and moisture permeability. At the same time, the tensile strength can reach up to 57.1 MPa, and has good mechanical properties. In addition, compared with Comparative Example 3, Example 7 has better waterproof and moisture permeability, indicating that the waterproof and moisture permeability of the fabrics prepared by introducing polyethylene oxide chain segments into the side chains of water-based polyurethane are better.

[0066] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A production process for waterproof and breathable fabric, characterized in that: The following steps are involved: S1, adding modified sodium alginate to the modified emulsion, stirring and mixing, to obtain a modified coating agent; S2. The polyester fabric is subjected to water repellent treatment, dipped and rolled, and after drying, the modified coating agent is evenly coated, and then dried to obtain a waterproof and breathable fabric.

2. The production process of a waterproof and breathable fabric according to claim 1, characterized in that: The weight ratio of the modified emulsion to the modified sodium alginate is 90-100:0.5-3.

3. The production process of a waterproof and breathable fabric according to claim 1, characterized in that: The coating thickness is 80-100 μm.

4. The production process of a waterproof and breathable fabric according to claim 1, characterized in that: The modified emulsion is prepared by the following steps: A1. Add 2,3-dihydroxysuccinic acid and polyethylene glycol monomethyl ether to toluene, stir to dissolve, add p-toluenesulfonic acid, reflux at 130-140° C. for 22-24 h, add excess anhydrous sodium bicarbonate, stir and mix for 30 min, filter, and then rotary evaporate the filtrate to obtain a modified polyether ester; A2. Under nitrogen protection, add poly(1,4-butylene adipate diol) to acetone, stir and mix, add modified polyether ester and isophorone diisocyanate, stir and mix, then drop stannous octoate, stir and react at 80-90°C for 3-4h, cool to 45-50°C, add trimethylolpropane, react at 70-75°C for 2-3h, cool to 20-25°C, and obtain a modified emulsion after post-treatment.

5. The production process of a waterproof and breathable fabric according to claim 4, characterized in that: The usage ratio of toluene, 2,3-dihydroxysuccinic acid, polyethylene glycol monomethyl ether and p-toluenesulfonic acid is 100 mL: 6-10 g: 15-21 mL: 0.5 g.

6. The production process of a waterproof and breathable fabric according to claim 4, characterized in that: The usage ratio of the acetone, poly(1,4-butylene adipate diol), modified polyether ester, isophorone diisocyanate, stannous octoate and trimethylolpropane is 80 mL: 14-21 g: 2-3 mL: 7-9 mL: 0.2 mL: 0.4-0.8 g.

7. The production process of a waterproof and breathable fabric according to claim 4, characterized in that: The post-treatment is to add deionized water, emulsify for 20-30 minutes, then dropwise add 0.3-0.5 wt % ethylenediamine aqueous solution, stir for 10 minutes, and then perform rotary evaporation.

8. The production process of a waterproof and breathable fabric according to claim 1, characterized in that: The modified sodium alginate is prepared by the following steps: Add sodium alginate to a phosphate buffer solution, stir to dissolve, add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, stir to mix, then add N-hydroxysuccinimide, stir to mix, then add octylamine, stir to react at 20-25° C. for 22-24 hours, then place in anhydrous ethanol for alcohol precipitation, centrifuge, wash, and dry to obtain modified sodium alginate.

9. The production process of a waterproof and breathable fabric according to claim 8, characterized in that: The dosage ratio of the phosphate buffer solution, sodium alginate, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and octylamine is 100 mL: 2-4 g: 0.5-1 g: 0.3-0.9 g: 0.8-1 mL; the pH value of the phosphate buffer solution is 5-6.

10. A waterproof and breathable fabric, characterized in that: Prepared according to the production process according to any one of claims 1 to 9.