Biolipid-based urethane acrylate adhesive as well as preparation method and application thereof

Through bio-greased polyurethane acrylate adhesive and high-energy electron beam irradiation technology, the problems of large odor, instability and high energy consumption in the production process of traditional adhesives are solved, and efficient and environmentally friendly textile printing adhesives are achieved. , improves the stability and performance of the adhesive.

CN118979397APending Publication Date: 2024-11-19JIANGSU NEW REBA TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411275529.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing acrylic adhesives have problems such as large odor, unstable production repeatability, formaldehyde residue and high energy consumption during the production process. The traditional chemical preparation method leads to uneven molecular weight of the adhesive and insufficient dry friction fastness.

Method used

Using bio-oil-based polyurethane acrylate adhesive, prepared by high-energy electron beam irradiation technology, combined with bio-based emulsifiers, natural oil sulfonated oils and lignin-furfural bio-based resins, to form a stable polymer adhesive to reduce Catalysts are used to improve molecular weight and bonding capacity.

Benefits of technology

It realizes an odorless, high stability, environmentally friendly and safe adhesive, improves the clarity of textile printing patterns, dry and wet friction fastness and low temperature resistance, reduces production energy consumption, and is suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005040055770000191
    Figure BDA0005040055770000191
  • Figure BDA0005040055770000201
    Figure BDA0005040055770000201
  • Figure BDA0005040055770000202
    Figure BDA0005040055770000202
Patent Text Reader

Abstract

The invention provides a biolipid-based urethane acrylate adhesive as well as a preparation method and application thereof. The biolipid-based urethane acrylate adhesive comprises the following components: biolipid-based urethane acrylate, a bio-based emulsifier, natural grease sulfonated oil, lignin-furfural bio-based resin and water, the biolipid-based polyurethane acrylate is prepared from the following raw materials in percentage by mass: 30%-40% of biolipid-based polyol, 40%-60% of isocyanate and 10%-20% of bio-based acrylate. The biolipid-based urethane acrylate adhesive provided by the invention is good in stability and odorless, and the preparation raw materials are mostly derived from bio-based products, so that the biolipid-based urethane acrylate adhesive is environment-friendly and safe; textile printed by the printing paste containing the biolipid-based urethane acrylate adhesive has clear pattern lines and high dry rubbing fastness and wet rubbing fastness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive materials, and in particular relates to a bio-oil-based polyurethane acrylate adhesive and a preparation method and application thereof. Background Art

[0002] Acrylic adhesives are mostly used in fields such as pigment printing on textiles. Whether the outline of the printed pattern is clear, dry friction fastness and wet friction fastness are important indicators for judging the quality of pigment printing adhesives.

[0003] CN102605648A discloses a water-based paint printing adhesive for textiles, wherein the weight ratio of raw materials of the water-based paint printing adhesive for textiles is: 33-35 acrylonitrile, 34-36 ethyl acrylate, 123-125 butyl acrylate, 3.5-4 acrylic acid, 3-3.5 hydroxyethyl methacrylate, 2-2.5 acrylamide, 1.5-1.75 sodium dodecyl sulfate, 6-7 dodecyl alcohol polyoxyethylene (10) ether, 300-310 deionized water, 0.8-0.9 ammonium persulfate, 0.4-0.45 sodium bisulfite, and the aqueous dispersion is formed after seed emulsion polymerization, and then mixed with a thermally deblocked polyurethane crosslinking agent at a ratio of 9-10:1 to obtain a paint printing adhesive. The product made of the water-based paint printing adhesive for textiles provided by the technical solution can be baked under low temperature conditions, and has good performance in terms of dry friction fastness, wet friction fastness, soaping fastness, etc., but the dry friction fastness still needs to be improved.

[0004] In addition, most of the raw materials in the traditional chemical method for preparing acrylic adhesives come from petroleum products, including emulsifiers. Emulsion polymerization often leads to unstable product particle size due to incorrect selection of emulsifiers, resulting in problems such as production blockage or product instability. During processing in the production workshop, there is a strong odor, which is not friendly to the working environment and operators, and affects the future use of textiles.

[0005] Currently, 90% of acrylic adhesives still use traditional reaction equipment for polymerization reaction, which is a reactor device heated by electricity, steam or electric oil. The chemical reaction time is long, and in addition to the acrylic reaction monomer, additional initiators, catalysts, molecular weight regulators, cross-linking agents, etc. must be added to trigger the polymerization reaction at a suitable temperature. It is impossible to completely remove formaldehyde residues, the molecular weight of the adhesive is uneven, and the production repeatability is unstable.

[0006] Now, gamma-ray irradiated acrylic adhesives have appeared in the technology. When Co60 decays, gamma rays are generated. Under the action of gamma rays, acrylic monomers undergo polymerization to generate polymer adhesives. The reaction time is shortened by half compared with traditional chemical adhesives. Gamma rays have strong penetrating power, so the particle size is relatively uniform and stable during the reaction, and the products produced are relatively stable. The production process is energy-saving and environmentally friendly. No auxiliary ingredients, such as initiators and catalysts, are added during the reaction. The ingredients are relatively clean and there is no formaldehyde residue. However, since the cobalt-60 source emits rays in a spherical shape, the utilization rate of the rays is low, only about 20%, and the rays in other directions are wasted.

[0007] In recent years, with the enhancement of people's environmental awareness and the improvement of national environmental laws and regulations, as well as the reduction of oil reserves and the price increase and environmental pollution caused by oil-based polymer materials, the adhesive industry needs to develop in the direction of safer, more environmentally friendly, energy-saving and cleaner production methods.

[0008] Therefore, it is necessary to develop a pigment printing adhesive for textiles with safe and environmentally friendly raw materials, energy-saving and cleaner preparation process, and better performance. Summary of the invention

[0009] In view of the shortcomings of the prior art, the present invention aims to provide a bio-oil-based polyurethane acrylate adhesive and a preparation method and application thereof. The bio-oil-based polyurethane acrylate adhesive has good stability and no odor, and its preparation raw materials are mostly derived from bio-based products, which can be completely biodegraded in the natural environment, and is environmentally friendly and safe; the textile pattern lines printed by the printing paste containing the bio-oil-based polyurethane acrylate adhesive are clear, and both dry friction fastness and wet friction fastness are high.

[0010] To achieve this object, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a bio-oil-based polyurethane acrylate adhesive, the bio-oil-based polyurethane acrylate adhesive comprising the following components: bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil, lignin-furfural bio-based resin and water;

[0012] The raw materials for preparing the bio-oil-based polyurethane acrylate include the following components by mass percentage: 30% to 40% (for example, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38% or 39%) of bio-oil-based polyol, 40% to 60% (for example, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56% or 58%) of isocyanate and 10% to 20% (for example, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% or 19%) of bio-based acrylate.

[0013] In the present invention, the bio-oil-based polyurethane acrylate adhesive is obtained by compounding bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil and lignin-furfural bio-based resin. The bio-oil-based polyurethane acrylate adhesive has good stability, no odor, high viscosity, and a small amount required for preparing printing paste. Most of the raw materials for its preparation are derived from bio-based products, and it can be completely biodegraded in the natural environment, which is environmentally friendly and safe. The printing paste containing the bio-oil-based polyurethane acrylate adhesive has good permeability and plasticity, and the printed textiles have bright patterns, clear lines, high color yield, uniform color, rich hand feel, high dry friction fastness and wet friction fastness, are resistant to low temperatures, fatigue-resistant, elastic, tough, and crease-free, can directly contact the human body, have no cytotoxicity, and are non-irritating to the skin, and are suitable for wide application.

[0014] In the present invention, the natural oil sulfonated oil is an anionic sulfonated oil fatting agent which is prepared by using natural oil as the main raw material, adopting sulfur trioxide gas sulfonation process for modification, and then compounding with other necessary components. The natural oil sulfonated oil is an excellent anionic surfactant, which improves the hydrophilic property and antistatic property; can reduce the friction between fabrics and between fibers, prevent fiber pilling, and improve the feel of the fabric surface.

[0015] In the present invention, the lignin-furfural bio-based resin is a furfural bio-based resin. Furfural is an important chemical raw material that can be prepared by bio-based conversion. Lignin is a biopolymer obtained from agricultural or forestry residues or paper pulping wastewater, and is the only aromatic natural biopolymer. Through enzymatic hydrolysis of lignin, the methoxyl group in lignin is demethylated and converted into a phenolic hydroxyl product to obtain a highly reactive nano-lignin. Furfural is used to completely replace formaldehyde, and reacts with highly reactive nano-lignin to synthesize lignin-furfural bio-based resin. It can cross-link the function of forming a network film on the fiber surface, so that the fiber surface is wrapped with a layer of wear-resistant resin film, the slip between fibers is reduced, and the yarn binding effect is good; at the same time, the lignin-furfural bio-based resin is uniformly cross-linked and condensed on the surface of the yarn, so that the fiber end adheres to the yarn, and it is not easy to pilling during friction. Improve the anti-pilling performance of the fabric and improve the anti-wrinkle, antistatic and other properties of the fabric. The bio-oil-based polyurethane acrylate adhesive improves the renewability and environmental friendliness of the product, and has significant social benefits and broad market prospects.

[0016] Preferably, the bio-oil-based polyurethane acrylate is prepared by the following method: dehydrating the bio-oil-based polyol, mixing it with isocyanate and bio-based acrylate, adding it into an irradiation tube to react under high-energy electron beam irradiation to obtain the bio-oil-based polyurethane acrylate.

[0017] In the present invention, the bio-oil-based polyurethane acrylate is prepared by reacting bio-oil-based polyol, isocyanate and bio-based acrylate under high-energy electron beam irradiation, and has high molecular weight and strong adhesion. The bio-based acrylate is derived from a chemical derivative of bio-based acrylic acid, produced using plant carbon, thereby increasing the renewable carbon content, having excellent properties such as ultra-low odor, low VOC, low emission and formaldehyde purification, and can replace traditional fossil carbon-based acrylates.

[0018] In the present invention, the production equipment of electron beam irradiation technology is used to replace the traditional chemical polymerization reactor to prepare bio-oil-based polyurethane acrylate, and the bio-oil-based polyol, isocyanate and bio-based acrylate are subjected to high-energy electron beam irradiation to undergo graft crosslinking and polymerization reaction to generate high-molecular bio-oil-based polyurethane acrylate, thereby reducing the use of catalysts. High-molecular irradiation crosslinking is to use high-energy ionizing radiation to induce polymer ionization and excitation to produce some secondary reactions, further form chemical reactions, and realize the formation of a crosslinked network between polymers. The process is simple, and the amount of electron beam irradiation emitted is controlled by a computer, reducing manual operation, controlling the reaction speed and temperature, and making the crosslinking and polymerization reactions uniform and continuous. Energy saving, high processing efficiency, irradiation processing energy consumption is only equal to 1 / 40 to 1 / 200 of thermal processing and chemical processing, and is 1 / 20 of freezing method, no environmental pollution, no chemical residues, no impurities will be introduced during the reaction process, and efficiency is improved, and there is no secondary pollution. The molecular weight of the polymer prepared by high-energy electron beam irradiation can be up to ten times that of the polymer prepared by traditional polymerization reactor polymerization. The prepared bio-oil-based polyurethane acrylate adhesive has stronger bonding ability and its usage in printing paste can be reduced by 20% to 40%. The higher molecular weight can also increase the fastness, and the printing process does not require high-temperature baking, but can use low-temperature baking, saving production energy consumption.

[0019] In the present invention, the low-temperature baking refers to baking at ≤130°C, and the high-temperature baking refers to baking at >130°C.

[0020] Preferably, the high-energy electron beam irradiation is performed using an electron beam emitting device.

[0021] It should be noted that the electron beam emitting device is also called an electron beam irradiation device or an electron accelerator. Electron beam irradiation technology is to use high-energy electron beams accelerated in a high-voltage electric field to irradiate substances, ionize and excite the molecules of various substances through the interaction between high-energy electrons and substances, thereby inducing chemical reactions to improve the performance of materials or generate new materials. It can have cross-linking, cracking, polymerization, grafting and other effects on substances, thereby producing physical, chemical or biological effects and achieving the purpose of radiation processing. Some processes that cannot be handled by heat or light can now be easily completed through electron beam irradiation, and the performance is very stable and the energy efficiency is very high. It takes into account the advantages of gamma-ray irradiation technology and has its own advantages. Because the accelerator has a large power, the energy of the rays is easy to control, the direction of the rays is in one direction, and the utilization rate of the rays is high, reaching more than 93%; the reaction time is greatly shortened compared to gamma-ray irradiation, and the irradiation reaction is completed in just a few minutes.

[0022] Preferably, the reaction is carried out under the condition of adding any one of inert gas, nitrogen or carbon dioxide gas after removing oxygen.

[0023] Preferably, the radiation dose rate of the high-energy electron beam irradiation is 1 to 20 kGy / h (for example, 2 kGy / h, 4 kGy / h, 6 kGy / h, 8 kGy / h, 10 kGy / h, 12 kGy / h, 14 kGy / h, 16 kGy / h or 18 kGy / h, etc.), further preferably 1 to 10 kGy / h, more preferably 1.5 to 2.5 kGy / h; the cumulative irradiation dose of the high-energy electron beam irradiation is 1 to 200 kGy (for example, 20 kGy, 40 kGy, 60 kGy, 80 kGy, 100 kGy, 120 kGy, 140 kGy, 160 kGy or 180 kGy, etc.), further preferably 10 to 100 kGy, more preferably 10 to 30 kGy.

[0024] Preferably, the feeding method of the high-energy electron beam irradiation is parallel and uniform speed continuous feeding of multiple irradiation tubes;

[0025] Preferably, the material viscosity of the feed is ≤10000mPa·s (for example, 1000mPa·s, 2000mPa·s, 3000mPa·s, 4000mPa·s, 5000mPa·s, 6000mPa·s, 7000mPa·s, 8000mPa·s or 9000mPa·s, etc.), and the feed speed is 2-7 kg / min (for example, 2.5 kg / min, 3 kg / min, 3.5 kg / min, 4 kg / min, 4.5 kg / min, 5 kg / min, 5.5 kg / min, 6 kg / min or 6.5 kg / min, etc.), and is further preferably 3-5 kg / min.

[0026] Preferably, the number of the irradiation tubes is 1-10 (for example, 2, 3, 4, 5, 6, 7, 8 or 9, etc.), and the inner diameter is 0.5-10 cm (for example, 1 cm, 2 cm, 3 cm, 4 cm, 5 cm, 6 cm, 7 cm, 8 cm or 9 cm, etc.).

[0027] Preferably, a cooling circulation system is installed under the irradiation tube, and the circulation speed of the cooling circulation system is 1-20 kg / min (for example, 2 kg / min, 4 kg / min, 6 kg / min, 8 kg / min, 10 kg / min, 12 kg / min, 14 kg / min, 16 kg / min or 18 kg / min, etc.), and more preferably 5-10 kg / min.

[0028] Preferably, the reaction temperature is ≤60°C, for example, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or 55°C, etc.

[0029] Preferably, the high-energy electron beam irradiation is carried out using an electron accelerator tube, the number of the electron accelerator tubes is 2-8 (for example, 3, 4, 5, 6 or 7, etc.), and the emission time interval is 0.2-1s (for example, 0.3s, 0.4s, 0.5s, 0.6s, 0.7s, 0.8s or 0.9s, etc.), and more preferably 0.3-0.5s.

[0030] In the present invention, the polymerization reaction of high-energy electron beam irradiation is an instantaneous and violent reaction, and a large amount of heat is released. Therefore, the single irradiation energy should not be too high. If the single irradiation energy is too high, the internal heat generated will not be discharged in time, and self-crosslinking will occur between monomers; and the penetration ability of the electron beam in the processed material is general. Therefore, in terms of the feeding method, multiple irradiation tubes are used for parallel and uniform continuous feeding, and the irradiation tubes are spread out and laid flat to increase the irradiation area and reduce the depth; reduce the radiation amount, increase the number of irradiation tubes, thereby increasing the number of irradiations, ensuring that the material reacts completely, and improving the conversion rate.

[0031] In the present invention, a cooling circulation system is installed under the irradiation tube to ensure that the material reaction temperature does not exceed 60°C, and the reaction chemical heat is taken away in time. The cooling area is the entire irradiation tube area. The circulation speed of the cooling circulation system is adjusted according to data such as material feeding speed, irradiation intensity, chemical reaction heat, etc.

[0032] Preferably, the isocyanate includes any one of 4,4'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, toluene diisocyanate, p-phenylene diisocyanate or cyclohexane diisocyanate, or a combination of at least two thereof, and more preferably toluene diisocyanate.

[0033] Preferably, the bio-based acrylate includes any one of hydroxyethyl methacrylate, pentaerythritol triacrylate, hydroxypropyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate or isooctyl acrylate, or a combination of at least two thereof, and more preferably hydroxypropyl acrylate.

[0034] Preferably, the bio-oil-based polyol is prepared by the following method:

[0035] (1) Bio-oil and bio-based acetic acid are mixed, concentrated sulfuric acid and hydrogen peroxide are added dropwise, reacted, and extracted to obtain epoxidized bio-oil.

[0036] (2) Mixing the epoxidized bio-oil obtained in step (1), lactic acid and a catalyst, removing oxygen and reacting to obtain a bio-oil-based polyol.

[0037] In the present invention, bio-oil is added into the reaction, epoxidized bio-oil is prepared by peracetic acid method, and then the bio-oil is ring-opened and epoxidized by lactic acid to prepare bio-oil-based polyol.

[0038] In the present invention, bio-oil, bio-based acrylate, bio-based emulsifier, natural oil sulfonated oil and lignin-furfural bio-based resin are all derived from natural raw materials, are non-toxic and harmless, are rapidly and thoroughly biodegraded, and do not pollute the environment; at the same time, the bio-oil-based polyurethane acrylate adhesive product has a mild effect, and the textiles are less damaged after treatment, which can achieve green and sustainable development of the industry.

[0039] Preferably, the biological oil comprises animal oil and / or vegetable oil, more preferably vegetable oil.

[0040] Preferably, the vegetable oil comprises any one of palm oil, palm kernel oil, soybean oil, peanut oil, sunflower oil or coconut oil, or a combination of at least two thereof, and palm oil is further preferred.

[0041] Preferably, the animal oil comprises lard and / or tallow.

[0042] In the present invention, the bio-oil is widely present in nature, and the refining process is relatively simple, so its price is relatively cheap, and the renewability and degradability of bio-oil are quite beneficial to the protection of the ecological environment. Palm oil is a kind of vegetable oil. Compared with rapeseed oil, castor oil, soybean oil, etc., it has abundant output, low price, wide application range, and the highest content of saturated fatty acids, the middle content of monounsaturated fatty acids, and the lowest content of polyunsaturated fatty acids. The saturated fatty acids and unsaturated fatty acids in its fatty acids account for about half each. The derivatives of palm oil can have good biodegradability and resource renewability, and contain double bonds that can be chemically modified to introduce active functional groups, making it an ideal monomer for synthesizing various polymers. The bio-oil-based polyols prepared from palmitic acid are more suitable as substitutes for petroleum-based polyols for the preparation of polyurethane acrylates, which have higher wear resistance, toughness, tear strength and low temperature resistance than the polyurethane acrylates prepared from petroleum-based polyols.

[0043] Preferably, the mass fraction of the concentrated sulfuric acid is 96% to 98%, for example, 96.2%, 96.4%, 96.6%, 96.8%, 97%, 97.2%, 97.4%, 97.6% or 97.8%.

[0044] Preferably, the mass fraction of the hydrogen peroxide is 20% to 25%, for example, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24% or 24.5%.

[0045] Preferably, during the process of adding concentrated sulfuric acid and hydrogen peroxide in step (1), the temperature of the control system is 30-40°C (for example, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C or 39°C, etc.), and the dropping time is 20-45min (for example, 23min, 26min, 29min, 32min, 35min, 38min, 41min or 44min, etc.).

[0046] In the present invention, during the process of adding concentrated sulfuric acid and hydrogen peroxide to the mixture of bio-oil and bio-based acetic acid, the temperature change of the system needs to be observed. If the temperature rises too fast, the dropping speed can be reduced.

[0047] Preferably, the reaction temperature in step (1) is 60-70°C (e.g., 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C or 69°C, etc.), and the reaction time is 5-8h (e.g., 5.5h, 6h, 6.5h, 7h or 7.5h, etc.).

[0048] Preferably, the extraction agent in step (1) is cyclohexane.

[0049] Preferably, in step (1), the mass ratio of the bio-oil, bio-acetic acid, hydrogen peroxide and concentrated sulfuric acid is 1: (0.1-0.5): (0.5-1.0): (0.002-0.010), for example, 1: 0.2: 0.6: 0.003, 1: 0.3: 0.6: 0.003, 1: 0.4: 0.6: 0.003, 1: 0.2: 0.7: 0.00 3. 1: 0.2: 0.8: 0.003, 1: 0.2: 0.9: 0.003, 1: 0.2: 0.6: 0.003, 1: 0.2: 0.6: 0.005, 1: 0.2: 0.6: 0.007 or 1: 0.2: 0.6: 0.009, etc., and more preferably 1: (0.25-0.3): (0.6-0.75): 0.005.

[0050] In the present invention, the mass ratio of the bio-oil, bio-based acetic acid, hydrogen peroxide and concentrated sulfuric acid is preferably 1: (0.25-0.3): (0.6-0.75): 0.005. The functionality of the bio-oil-based polyol obtained by ring opening of the prepared epoxidized bio-oil is about 2, that is, 1 mol of the bio-oil-based polyol contains about 2 mol of hydroxyl groups.

[0051] Preferably, the epoxy value of the epoxidized bio-grease is 1.9% to 2.3%, such as 1.95%, 2.0%, 2.05%, 2.1%, 2.15%, 2.2% or 2.25%.

[0052] Preferably, the reaction temperature in step (2) is 90-100°C (e.g., 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C or 99°C, etc.), and the reaction time is 5-8h (e.g., 5.5h, 6h, 6.5h, 7h or 7.5h, etc.).

[0053] Preferably, the catalyst in step (2) is triphenylphosphine.

[0054] Preferably, the mass of the catalyst in step (2) is 0.5% to 2% of the total mass of lactic acid and epoxidized bio-oil, for example, 0.7%, 0.9%, 1.1%, 1.3%, 1.5%, 1.7% or 1.9%, etc.

[0055] Preferably, the molar ratio of the carboxylic acid in the lactic acid to the epoxy group in the epoxidized bio-oil in step (2) is (2-7):1, such as 2:1, 3:1, 4:1, 5:1 or 6:1, and more preferably (4-6):1.

[0056] In the present invention, the molar ratio of the carboxylic acid in the lactic acid to the epoxy group in the epoxidized bio-oil is preferably (4-6):1, whereby the conversion rate of the epoxy group to the hydroxyl group increases and may exceed 85%.

[0057] Preferably, the bio-based emulsifier comprises any one or a combination of at least two of palm kernel oil ethoxylate sodium sulfonate, modified palm kernel oil ethoxylate or modified soybean oil ethoxylate, and more preferably palm kernel oil ethoxylate sodium sulfonate and modified palm kernel oil ethoxylate.

[0058] Preferably, the mass ratio of the sodium palm kernel oil ethoxylate sulfonate to the modified palm kernel oil ethoxylate is (1.1-1.3):(1.1-1.3), for example, 1.1:1.2, 1.1:1.3, 1.2:1.3, 1.2:1.2 or 1.3:1.2, etc.

[0059] Preferably, the sodium palm kernel oil ethoxylate sulfonate is SNS80.

[0060] Preferably, the modified palm kernel oil ethoxylate is SOE-N-60.

[0061] Preferably, the natural fat sulfonated oil includes any one of natural sulfonated rapeseed oil, natural sulfonated castor oil or sulfated natural neatsfoot oil, or a combination of at least two thereof, and more preferably natural sulfonated rapeseed oil.

[0062] In the present invention, the natural fat sulfonated oil is an anionic surfactant, and the bio-based emulsifier is a nonionic surfactant, and the two work together to make each component evenly dispersed in the emulsion.

[0063] Preferably, the mass ratio of the natural sulfonated rapeseed oil, the sodium palm kernel oil ethoxylate sulfonate and the modified palm kernel oil ethoxylate is 1:(1.1-1.3):(1.1-1.3), for example, 1:1.1:1.2, 1:1.1:1.3, 1:1.2:1.3, 1:1.2:1.2 or 1:1.3:1.2, etc.

[0064] Preferably, the bio-oil-based polyurethane acrylate adhesive further comprises the following components: a pH regulator and a defoaming agent.

[0065] Preferably, the pH adjuster includes any one of aqueous ammonia, liquid alkali or organic alkali, or a combination of at least two of them.

[0066] Preferably, the defoaming agent comprises polyoxypropyl polyoxyethyl glyceryl ether and / or polyether-modified polysiloxane defoaming agent.

[0067] Preferably, the raw materials for preparing the bio-oil-based polyurethane acrylate adhesive include the following components by mass percentage: 11% to 40% (e.g., 15%, 18%, 21%, 24%, 27%, 33%, 36% or 39%) of bio-oil-based polyurethane acrylate, 1% to 5% (e.g., 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%) of bio-based emulsifier, 1% to 5% (e.g., 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%) of natural oil sulfonated oil, 5% to 15% (e.g., 6% to 10% of lignin-furfural bio-based resin). %, 7%, 8%, 9%, 10%, 11%, 12%, 13% or 14%, etc.), pH adjuster 0.01% to 1% (for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8% or 0.9%, etc.), defoaming agent 0.01% to 0.5% (for example, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4% or 0.45%, etc.) and water 40% to 82% (for example, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc.).

[0068] In a second aspect, the present invention provides a method for preparing the bio-oil-based polyurethane acrylate adhesive as described in the first aspect, the preparation method comprising the following steps: mixing bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil, lignin-furfural bio-based resin and water to obtain the bio-oil-based polyurethane acrylate adhesive.

[0069] Preferably, the preparation method specifically comprises the following steps: mixing bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil, lignin-furfural bio-based resin and water in a first step, then adding a pH regulator and a defoaming agent in a second step, filtering the material, and obtaining the bio-oil-based polyurethane acrylate adhesive.

[0070] Preferably, the first mixing temperature is 40-60°C, for example, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C or 58°C.

[0071] Preferably, the temperature of the second mixing is 0-45°C, for example, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C or 40°C.

[0072] In a third aspect, the present invention provides a printing paste, wherein the printing paste comprises the bio-oil-based polyurethane acrylate adhesive as described in the first aspect.

[0073] Preferably, the printing paste comprises the following components by mass percentage: 10% to 30% (for example, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26% or 28%) of bio-oil-based polyurethane acrylate adhesive, 2% to 10% (for example, 3%, 4%, 5%, 6%, 7%, 8% or 9%) of moisturizer, 1% to 5% (for example, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%) of pigment, 1% to 5% (for example, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%) of thickener and 50% to 86% (for example, 55%, 60%, 65%, 70%, 75%, 80% or 85%) of water.

[0074] Preferably, the humectant comprises urea.

[0075] Preferably, the thickener comprises an acrylic thickener.

[0076] Preferably, the printing paste comprises the following components by mass percentage: 10% to 20% (e.g., 12%, 14%, 16%, 18% or 20%) of bio-oil-based polyurethane acrylate adhesive, 8% to 10% (e.g., 8.2%, 8.4%, 8.6%, 8.8%, 9%, 9.2%, 9.4%, 9.6% or 9.8%) of moisturizer, 2% to 3% (e.g., 2.1%, 2. 2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8% or 2.9%, etc.), thickener 2% to 3% (for example, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8% or 2.9%, etc.) and water 60% to 80% (for example, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76% or 78%, etc.).

[0077] In a fourth aspect, the present invention provides an application of the printing paste as described in the third aspect on cloth printing, and the application comprises the following steps: printing the printing paste as described in the third aspect on cloth, drying, baking or steaming to obtain printed cloth.

[0078] Preferably, the baking temperature is 110-130°C (for example, 112°C, 114°C, 116°C, 118°C, 120°C, 122°C, 124°C, 126°C or 128°C, etc.), and the time is 1-2min (for example, 1.1min, 1.2min, 1.3min, 1.4min, 1.5min, 1.6min, 1.7min, 1.8min or 1.9min, etc.).

[0079] Preferably, the fabric comprises poplin fabric.

[0080] Compared with the prior art, the present invention has the following beneficial effects:

[0081] The bio-oil-based polyurethane acrylate adhesive of the present invention is obtained by compounding the bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil and lignin-furfural bio-based resin. The bio-oil-based polyurethane acrylate adhesive has good stability, no odor, high viscosity, and a small amount required for preparing printing paste. Most of the raw materials for its preparation are derived from bio-based products, and it can be completely biodegraded in the natural environment, which is environmentally friendly and safe. The printing paste prepared by the bio-oil-based polyurethane acrylate adhesive has good permeability and plasticity, and the printed textiles have bright patterns, clear lines, high color yield, uniform color, rich hand feel, high dry friction fastness and wet friction fastness, are resistant to low temperatures, fatigue-resistant, elastic, tough, and crease-free, can directly contact the human body, have no cytotoxicity, are non-irritating to the skin, and are suitable for wide application. DETAILED DESCRIPTION

[0082] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0083] The sources of some components in the embodiments and comparative examples are as follows:

[0084] Bio-based acetic acid, Swiss CleanTech;

[0085] Sodium palm kernel oil ethoxylate sulfonate, brand name SNS80;

[0086] Modified palm kernel oil ethoxylate, brand name SOE-N-60;

[0087] Natural sulfonated rapeseed oil, Qingdao Incoline Biotechnology;

[0088] Lignin-furfural bio-based resin, prepared according to Example 1 of CN116063643A;

[0089] Liquid caustic soda: aqueous solution of NaOH, in which the mass percentage of NaOH is 32.5%;

[0090] Polyether modified polysiloxane defoamer, manufacturer: Chengda (Shanghai) Chemical, brand name: CD-1116M.

[0091] Preparation Example 1

[0092] This preparation example provides a bio-oil-based polyurethane acrylate, specifically bio-oil-based polyurethane acrylate A, which is prepared by the following method:

[0093] Preparation of bio-oil based polyols:

[0094] (1) 2000g of bio-oil (palm oil) and 500g of bio-acetic acid were mechanically mixed uniformly, and 10g of concentrated sulfuric acid (mass fraction 96%) and 1500g of hydrogen peroxide (mass fraction 20%) were added dropwise under mechanical stirring, and the temperature of the system was controlled within the range of 30-40°C by the dropping speed during the dropping process, and the dropping time was 30min; after reacting at 60°C for 6h, the mixture was cooled to room temperature. The mixture was extracted with cyclohexane and washed with deionized water until the lower clear liquid after stratification was neutral, the organic layer was collected, the cyclohexane was recovered by heating at normal pressure, and the small molecules were removed by decompression to obtain epoxidized bio-oil, and the epoxide value of the epoxidized bio-oil was 2.0%.

[0095] (2) Add 2000 g of the epoxidized bio-oil obtained in step (1) and 360 g of lactic acid into a pressure-resistant reactor, configure a mechanical stirrer, add 23.6 g of a catalyst (triphenylphosphine) after removing oxygen, and heat to 95° C. After reacting for 6 h and waiting for the reaction pressure to no longer change, mature for 1 h and then vacuum remove the residual monomers. After the reaction temperature cools to room temperature, wash the product with deionized water until it is neutral, and remove water in the system under reduced pressure to obtain a bio-oil-based polyol.

[0096] Preparation of bio-oil-based polyurethane acrylate:

[0097] 2000g of the above-mentioned bio-oil-based polyol was dehydrated in a pressure-resistant reactor at 100°C using a vacuum oil pump. After no obvious bubbles emerged, 2500g of toluene diisocyanate and 500g of hydroxypropyl acrylate were added and mixed evenly. Then, the mixture was added to the irradiation tube at 25°C at a feeding rate of 2.5 kg / min. The feeding method was continuous feeding of the irradiation tube. Nitrogen was added to the irradiation tube after oxygen was removed. The number of the irradiation tubes was 1 and the inner diameter was 0.5 cm. The irradiation tubes were irradiated with a high-energy electron beam. The reaction is carried out under the conditions of 200 ° C., the high-energy electron beam irradiation is carried out by an electron accelerator tube, the number of the electron accelerator tubes is 2, the emission time interval is 0.3s, a cooling circulation system is installed under the irradiation tube, the circulation speed of the cooling circulation system is 5 kg / min, the reaction temperature of the material is controlled to be 50 ° C, the radiation dose rate of the high-energy electron beam irradiation is 2 kGy / h, the cumulative irradiation dose of the high-energy electron beam irradiation is 10 kGy, and a vacuum oil pump is used for degassing to obtain bio-oil-based polyurethane acrylate A.

[0098] Preparation Example 2

[0099] This preparation example provides a bio-oil-based polyurethane acrylate, specifically bio-oil-based polyurethane acrylate B, which differs from Preparation Example 1 only in that, in the preparation of bio-oil-based polyurethane acrylate, the mass of bio-oil-based polyol is adjusted to 1500 g, and the mass of hydroxypropyl acrylate is adjusted to 1000 g, and other conditions are the same as those in Preparation Example 1.

[0100] Preparation Example 3

[0101] This preparation example provides a bio-oil-based polyurethane acrylate, specifically bio-oil-based polyurethane acrylate C, which differs from Preparation Example 1 only in that, in the preparation of the bio-oil-based polyurethane acrylate, the mass of the bio-oil-based polyol is adjusted to 1250 g, and the mass of hydroxypropyl acrylate is adjusted to 1250 g, and the other conditions are the same as those in Preparation Example 1.

[0102] Example 1

[0103] The present embodiment provides a bio-oil-based polyurethane acrylate adhesive and a preparation method thereof. The raw materials for preparing the bio-oil-based polyurethane acrylate adhesive include the following components in percentage by mass: 25% of the bio-oil-based polyurethane acrylate provided in Preparation Example 1, 2.2% of sodium palm kernel oil ethoxylate sulfonate (SNS80), 2.2% of modified palm kernel oil ethoxylate (SOE-N-60), 2% of natural sulfonated rapeseed oil, 10% of lignin-furfural bio-based resin, 0.3% of liquid alkali, 0.5% of polyether-modified polysiloxane defoamer (CD-1116M) and 57.8% of water.

[0104] The preparation method of the bio-grease-based polyurethane acrylate adhesive is as follows:

[0105] Add water to the reactor, start stirring, raise the temperature to 50°C, add the bio-oil-based polyurethane acrylate, sodium palm kernel oil ethoxylate sulfonate, modified palm kernel oil ethoxylate, natural sulfonated rapeseed oil, and lignin-furfural bio-based resin provided in Preparation Example 1, stir and mix thoroughly; then add liquid alkali and polyether-modified polysiloxane defoamer and mix at 30°C, filter the material, and obtain the bio-oil-based polyurethane acrylate adhesive.

[0106] Example 2

[0107] The present embodiment provides a bio-oil-based polyurethane acrylate adhesive and a preparation method thereof. The raw materials for preparing the bio-oil-based polyurethane acrylate adhesive include the following components in percentage by mass: 35% of the bio-oil-based polyurethane acrylate provided in Preparation Example 1, 2.2% of sodium palm kernel oil ethoxylate sulfonate (SNS80), 2.2% of modified palm kernel oil ethoxylate (SOE-N-60), 2% of natural sulfonated rapeseed oil, 5% of lignin-furfural bio-based resin, 0.3% of liquid alkali, 0.5% of polyether-modified polysiloxane defoamer (CD-1116M) and 52.8% of water.

[0108] The preparation method of the bio-grease-based polyurethane acrylate adhesive is as follows:

[0109] Add water to the reactor, start stirring, raise the temperature to 50°C, add the bio-oil-based polyurethane acrylate, sodium palm kernel oil ethoxylate sulfonate, modified palm kernel oil ethoxylate, natural sulfonated rapeseed oil, and lignin-furfural bio-based resin provided in Preparation Example 1, stir and mix thoroughly; then add liquid alkali and polyether-modified polysiloxane defoamer and mix at 30°C, filter the material, and obtain the bio-oil-based polyurethane acrylate adhesive.

[0110] Example 3

[0111] This embodiment provides a bio-oil-based polyurethane acrylate adhesive and a preparation method thereof, which differs from Example 2 only in that the bio-oil-based polyurethane acrylate provided in Preparation Example 1 is replaced with the bio-oil-based polyurethane acrylate provided in Preparation Example 2 of the same mass, and other conditions are the same as in Example 2.

[0112] Example 4

[0113] This embodiment provides a bio-oil-based polyurethane acrylate adhesive and a preparation method thereof, which differs from Example 2 only in that the bio-oil-based polyurethane acrylate provided in Preparation Example 1 is replaced with the bio-oil-based polyurethane acrylate provided in Preparation Example 3 of the same mass, and other conditions are the same as in Example 2.

[0114] Example 5

[0115] This embodiment provides a bio-oil-based polyurethane acrylate adhesive and a preparation method thereof, which is different from Example 2 only in that the mass percentage of the bio-oil-based polyurethane acrylate is adjusted to 30%, and the mass percentage of the lignin-furfural bio-based resin is adjusted to 10%, and other conditions are the same as Example 2.

[0116] Example 6

[0117] The present embodiment provides a bio-oil-based polyurethane acrylate adhesive and a preparation method thereof, which differs from Example 2 only in that the preparation example 1 provides 35% of bio-oil-based polyurethane acrylate, 2.6% of sodium palm kernel oil ethoxylate sulfonate (SNS80), 2.6% of modified palm kernel oil ethoxylate (SOE-N-60), 5% of natural sulfonated rapeseed oil, 5% of lignin-furfural bio-based resin, 0.3% of liquid alkali, 0.2% of polyether-modified polysiloxane defoamer (CD-1116M) and 49.3% of water, and other conditions are the same as those in Example 2.

[0118] Comparative Example 1

[0119] This comparative example provides a waterborne polyurethane textile coating resin, which is a commercially available waterborne polyurethane textile coating resin HY517.

[0120] Comparative Example 2

[0121] This comparative example provides an adhesive and a preparation method thereof, which differs from Example 2 only in that no bio-oil-based polyurethane acrylate is added, the mass percentage of lignin-furfural bio-based resin is adjusted to 40%, and other conditions are the same as Example 2.

[0122] Comparative Example 3

[0123] This comparative example provides an adhesive and a preparation method thereof, which differs from Example 2 only in that no lignin-furfural bio-based resin is added, the mass percentage of bio-oil-based polyurethane acrylate is adjusted to 40%, and other conditions are the same as Example 2.

[0124] Comparative Example 4

[0125] This comparative example provides an adhesive and a preparation method thereof, which differs from Example 2 only in that no natural fat sulfonated oil is added, the mass percentage of water is adjusted to 54.8%, and other conditions are the same as those in Example 2.

[0126] Application Example 1

[0127] This application example provides a printing paste and a printing fabric, comprising 15% of the bio-oil-based polyurethane acrylate adhesive provided in Example 1, 8% of a moisturizer (urea), 3% of a pigment (pigment blue 60), 4% of a thickener (acrylic thickener, Guangzhou Hengyu Chemical, ASE-60) and 70% of water.

[0128] The printed fabric is prepared by the following method:

[0129] 4 g of thickener and 70 g of water were mixed, stirred for 5 min to disperse evenly, the stirring speed was 50 rpm, and the mixture was allowed to stand for 20 min. Then, 15 g of bio-oil-based polyurethane acrylate adhesive, 3 g of pigment, and 8 g of moisturizer were added in sequence, and the mixture was stirred for 5 min to form a printing slurry. The printing slurry was then poured into a printing screen, and the printing slurry was quickly scraped from top to bottom with a rubber scraper. The printing slurry flowed down from the screen and transferred to a poplin fabric to print a desired pattern. The printed fabric was dried at 100° C. for 2 min, and then baked on a setting machine for color fixation. The baking temperature was 130° C. and the time was 1.5 min to obtain the printed fabric.

[0130] Application Examples 2 to 6

[0131] Application Examples 2 to 6 provide a printing paste and a printed fabric, which differ from Application Example 1 only in that the bio-oil-based polyurethane acrylate adhesive provided in Example 1 is replaced by the bio-oil-based polyurethane acrylate adhesive provided in Examples 2 to 6, respectively, and other conditions are the same as those in Application Example 1.

[0132] Comparative Application Examples 1 to 4

[0133] Comparative Application Examples 1 to 4 provide a printing paste and a printed fabric, which differ from Application Example 1 only in that the bio-oil-based polyurethane acrylate adhesive provided in Example 1 is replaced by the water-based polyurethane textile coating resin provided in Comparative Example 1 and the adhesive provided in Comparative Examples 2 to 4, respectively, and other conditions are the same as those in Application Example 1.

[0134] Performance Testing

[0135] (1) Adhesion test: The bio-oil-based polyurethane acrylates provided in Preparation Examples 1 to 3 were mixed with water to prepare a mixed solution with a solid content of 35%, so that the solid content was the same as that of the water-based polyurethane textile coating resin provided in Comparative Example 1, and then tested in accordance with the national standard GB / T 6739-2006 "Determination of film hardness by pencil method for paints and varnishes", using a Zhonghua brand QHQ-B pencil hardness tester. The rating standard is shown in Table 1, and the test results are shown in Table 2.

[0136] Table 1

[0137]

[0138] (2) Flat screen printing fastness performance test: The printed positions of the printed fabrics provided in Application Examples 1 to 6 and Comparative Application Examples 1 to 4 were tested for dry and wet friction fastness. The test method was carried out in accordance with ISO 105-X12-2016 standard. The higher the rating, the better the fastness. The test results are shown in Table 3.

[0139] (3) Leveling and flow properties test: Observe whether the printed pattern outlines at the printing positions of the printed fabrics provided in Application Examples 1 to 6 and Comparative Application Examples 1 to 4 are distinct, whether the patterns are clear, and whether the colors are bright and uniform. The clearer the edges of the pattern effects, the better the leveling and flow properties of the printing paste. The test results are shown in Table 3.

[0140] (4) Hand feel evaluation: The softness and smoothness of the printed fabrics were evaluated by hand touch. The scores were averaged by five testers. The hand feel of poplin fabric was rated as level 1. The larger the value, the better the hand feel. The best hand feel was rated as level 5; greater than level 2 and less than level 3 was rated as level 2-3; greater than level 3 and less than level 4 was rated as level 3-4; greater than level 4 and less than level 5 was rated as level 4-5.

[0141] Table 2

[0142]

[0143] Table 3

[0144]

[0145]

[0146] The bio-oil-based polyurethane acrylate adhesive product provided in Examples 1-6 is stable, in the form of a transparent viscous liquid, has a solid content in the range of 30% to 51%, a pH of 6-8, is non-toxic, non-corrosive, has no irritating odor, and has good safety. The bio-oil-based polyurethane acrylate adhesive provided by the present invention is an adhesive that can be used for textile processing, has high safety, and has good application prospects.

[0147] Comparing Preparation Example 1 with Preparation Example 2, it can be seen from Table 2 that if the content of bio-oil-based polyol is high, the prepared bio-oil-based polyurethane acrylate has the same adhesion to stone plastic board, glass and steel plate, better adhesion to tinplate, wood board and PET film, and better overall adhesion. The higher the content of bio-oil-based polyol, the better the toughness of the prepared bio-oil-based polyurethane acrylate, and the more elastic the formed film. Comparing Application Example 2 with Application Example 3, it can be seen from Table 3 that if the content of bio-based acrylate is high, the dry friction fastness of the printed position of the prepared printed fabric is higher, the dry friction fastness is the same, and the overall friction fastness is better.

[0148] Compared with Preparation Example 1, the adhesion of the waterborne polyurethane textile coating resin HY517 (Comparative Example 1) to glass is lower.

[0149] Compared with Application Example 2, the dry friction fastness and wet friction fastness of the printed position of the printed fabric prepared by adding the water-based polyurethane textile coating resin HY517 (Comparative Application Example 1) are both low. The performance of the bio-oil-based polyurethane acrylate adhesive provided by the present invention is better than that of the traditional water-based polyurethane adhesive.

[0150] Compared with Application Example 2, if bio-oil-based polyurethane acrylate is not added to the adhesive (Comparative Application Example 2), the rubbing fastness grades of both dry rubbing fastness and wet rubbing fastness are greatly reduced, and cannot meet the requirements for textile printing.

[0151] Compared with Application Example 2, if the lignin-furfural bio-based resin is not added to the adhesive (Comparative Application Example 3), the rubbing fastness grade of the wet rubbing fastness decreases.

[0152] Compared with Application Example 2, if the natural fat sulfonated oil is not added to the adhesive (Comparative Application Example 4), the friction fastness grades of the dry friction fastness and the wet friction fastness decrease, and the hand feel becomes worse.

[0153] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate a bio-oil-based polyurethane acrylate adhesive and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A bio-oil-based polyurethane acrylate adhesive, It is characterized in that The bio-oil-based polyurethane acrylate adhesive comprises the following components: bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil, lignin-furfural bio-based resin and water; The raw materials for preparing the bio-oil-based polyurethane acrylate include the following components by mass percentage: 30% to 40% of bio-oil-based polyol, 40% to 60% of isocyanate and 10% to 20% of bio-based acrylate.

2. The bio-oil-based polyurethane acrylate adhesive according to claim 1, It is characterized in that The bio-oil-based polyurethane acrylate is prepared by the following method: dehydrating the bio-oil-based polyol, mixing it with isocyanate and bio-based acrylate, adding it into an irradiation tube to react under high-energy electron beam irradiation to obtain the bio-oil-based polyurethane acrylate; Preferably, the reaction is carried out under the condition of adding any one of inert gas, nitrogen or carbon dioxide gas after removing oxygen; Preferably, the radiation dose rate of the high-energy electron beam irradiation is 1 to 20 kGy / h, and the cumulative irradiation dose is 1 to 200 kGy; Preferably, the reaction temperature is ≤60°C; Preferably, the isocyanate includes any one or a combination of at least two of 4,4'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, toluene diisocyanate, p-phenylene diisocyanate or cyclohexane diisocyanate; Preferably, the bio-based acrylate includes any one of hydroxyethyl methacrylate, pentaerythritol triacrylate, hydroxypropyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate or isooctyl acrylate, or a combination of at least two thereof.

3. The bio-oil-based polyurethane acrylate adhesive according to any one of claims 1 to 2, It is characterized in that The bio-oil-based polyol is prepared by the following method: (1) mixing bio-oil and bio-based acetic acid, adding concentrated sulfuric acid and hydrogen peroxide dropwise, reacting, extracting, and obtaining epoxidized bio-oil; (2) mixing the epoxidized bio-oil obtained in step (1), lactic acid and a catalyst, removing oxygen and reacting to obtain a bio-oil-based polyol; Preferably, the bio-oil comprises animal oil and / or vegetable oil; Preferably, the vegetable oil comprises any one of palm oil, palm kernel oil, soybean oil, peanut oil, sunflower seed oil or coconut oil, or a combination of at least two thereof; Preferably, the animal oil comprises lard and / or tallow; Preferably, in the process of adding concentrated sulfuric acid and hydrogen peroxide in step (1), the temperature of the system is controlled to be 30-40° C., and the adding time is 20-45 min; Preferably, the reaction temperature in step (1) is 60-70° C., and the reaction time is 5-8 h; Preferably, the extraction agent in step (1) is cyclohexane; Preferably, the mass ratio of the bio-oil, bio-based acetic acid, hydrogen peroxide and concentrated sulfuric acid in step (1) is 1: (0.1-0.5): (0.5-1.0): (0.002-0.010); Preferably, the epoxy value of the epoxy bio-grease is 1.9% to 2.3%; Preferably, the reaction temperature in step (2) is 90-100° C., and the reaction time is 5-8 h; Preferably, the catalyst in step (2) is triphenylphosphine; Preferably, the mass of the catalyst in step (2) is 0.5% to 2% of the total mass of lactic acid and epoxidized bio-oil; Preferably, in step (2), the molar ratio of the carboxylic acid in the lactic acid to the epoxy group in the epoxidized bio-oil is (2-7):

1.

4. The bio-oil-based polyurethane acrylate adhesive according to any one of claims 1 to 3, It is characterized in that The bio-based emulsifier includes any one or a combination of at least two of palm kernel oil ethoxylate sodium sulfonate, modified palm kernel oil ethoxylate or modified soybean oil ethoxylate, and more preferably palm kernel oil ethoxylate sodium sulfonate and modified palm kernel oil ethoxylate; Preferably, the mass ratio of the palm kernel oil ethoxylate sodium sulfonate to the modified palm kernel oil ethoxylate is (1.1-1.3): (1.1-1.3); Preferably, the natural fat sulfonated oil includes any one of natural sulfonated rapeseed oil, natural sulfonated castor oil or sulfated natural neatsfoot oil, or a combination of at least two thereof.

5. The bio-oil-based polyurethane acrylate adhesive according to any one of claims 1 to 4, It is characterized in that The bio-oil-based polyurethane acrylate adhesive further comprises the following components: a pH regulator and a defoamer; Preferably, the pH adjuster comprises any one or a combination of at least two of ammonia water, liquid alkali or organic alkali; Preferably, the defoaming agent comprises polyoxypropyl polyoxyethyl glycerol ether and / or polyether-modified polysiloxane defoaming agent; Preferably, the raw materials for preparing the bio-oil-based polyurethane acrylate adhesive include the following components by mass percentage: 11% to 40% bio-oil-based polyurethane acrylate, 1% to 5% bio-based emulsifier, 1% to 5% natural oil sulfonated oil, 5% to 15% lignin-furfural bio-based resin, 0.01% to 1% pH adjuster, 0.01% to 0.5% defoamer and 40% to 82% water.

6. A method for preparing the bio-oil-based polyurethane acrylate adhesive according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: mixing bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil, lignin-furfural bio-based resin and water to obtain the bio-oil-based polyurethane acrylate adhesive.

7. The preparation method according to claim 6, It is characterized in that The preparation method specifically comprises the following steps: firstly mixing bio-oil-based polyurethane acrylate, bio-based emulsifier, natural oil sulfonated oil, lignin-furfural bio-based resin and water, then adding pH regulator and defoamer for second mixing, filtering the material, and obtaining the bio-oil-based polyurethane acrylate adhesive; Preferably, the temperature of the first mixing is 40-60°C; Preferably, the temperature of the second mixing is 0-45°C.

8. A printing paste, It is characterized in that The printing paste comprises the bio-oil-based polyurethane acrylate adhesive as described in any one of claims 1-5.

9. The printing paste according to claim 8, It is characterized in that The printing paste comprises the following components by mass percentage: 10% to 30% of bio-oil-based polyurethane acrylate adhesive, 2% to 10% of moisturizer, 1% to 5% of pigment, 1% to 5% of thickener and 50% to 86% of water; Preferably, the humectant comprises urea; Preferably, the thickener comprises an acrylic thickener.

10. Use of the printing paste as claimed in claim 8 or 9 for printing on cloth, It is characterized in that The application comprises the following steps: printing the printing paste as claimed in claim 8 or 9 on cloth, drying, baking or steaming to obtain printed cloth; Preferably, the baking temperature is 110-130° C. and the baking time is 1-2 min.

Citation Information

Patent Citations

  • Textile water-based pigment printing binding agent and preparation method

    CN102605648A

  • Lignin-furfural biomass-based phenolic resin as well as preparation method and application thereof

    CN116063643A