Water-based lubricant for papermaking coating and application of water-based lubricant

By using water-based lubricants with water-based oxidized polyethylene copolymer and other components during papermaking coating, the problem of poor fluidity of the coating is solved, and paper diseases such as streaks and orange peel are reduced, and the smoothness of the paper is improved. Lubricating performance adapts to the demand for high-solid content coatings and reduces production costs.

CN118979407AActive Publication Date: 2024-11-19DONGGUAN NINE DRAGONS PAPER IND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411083586.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The poor fluidity of the paint during the existing papermaking coating process leads to paper diseases such as stripes, orange peels, and roll marks. The lubricating performance of high-solid content coatings is insufficient, making it difficult to meet the production requirements of high-speed coating paper machines.

Method used

Using an aqueous lubricant, including aqueous oxidized polyethylene copolymer, surfactant, bactericide and initiator, a high solids content of water-based lubricant is prepared through specific ratios and preparation methods to improve the fluidity of the coating and Leveling, reduce the friction coefficient of the coating and improve the gloss of the paper.

Benefits of technology

Effectively improve the fluidity and leveling of the coating, reduce the phenomenon of hair loss and powder loss during coating cracking and printing, improve the smoothness of the paper surface, and is suitable for high-solid content coatings, which are low-cost and suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984508880000141
    Figure BDA0004984508880000141
  • Figure BDA0004984508880000151
    Figure BDA0004984508880000151
Patent Text Reader

Abstract

The invention provides a water-based lubricant for papermaking coating and application of the water-based lubricant. The water-based lubricant for papermaking coating comprises the following components in parts by weight: 13-18 parts of a water-based oxidized polyethylene copolymer, 3-8 parts of a surfactant, 5-7 parts of a bactericide, 10-12 parts of an initiator and 100 parts of water, the preparation method of the water-based oxidized polyethylene copolymer comprises the following steps: (1) mixing ethylene oxide and oxidized polyethylene, and then sequentially carrying out mixing reaction and standing to obtain a reaction solution; and (2) mixing amide and the reaction liquid, and carrying out a modification reaction to obtain the water-based oxidized polyethylene copolymer. The lubricant provided by the invention solves the problem of poor fluidity in the coating process, and reduces or even avoids streaks, orange peels and rolling marks in the coating process; the phenomena of shrinkage cavities, needle eye sagging and the like occur in the drying process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lubricants and relates to a paper coating lubricant, in particular to a water-based lubricant for papermaking coating and application thereof. Background Art

[0002] As the production scale of the domestic papermaking industry continues to expand, the demand for coated paper continues to increase, and the speed of coated paper machines is getting faster and faster. The fluidity of the coating during the coating process is the key to uniform coating. Each coating has a fixed point, and the fixed points of coatings of different properties or different coating components are also different. The fixed point of the coating is generally within the range of 80% to 87% solid content, and the leveling phenomenon can only be completed before the coating reaches the fixed point during the drying process. The leveling phenomenon produces a regular flow phenomenon; with the evaporation of the solvent, a higher surface tension is formed on the surface of the coating film, and the viscosity increases. At the same time, the temperature drops; resulting in a temperature difference between the inner and outer layers and a difference in surface tension and viscosity, poor leveling, and streaks, orange peels, and rolling marks will appear during application; shrinkage holes, pinholes, and sagging will appear during the drying process. In order to avoid paper diseases caused by poor coating fluidity during the coating process, it is necessary to enhance the fluidity of the coating.

[0003] This makes the lubrication performance of the coating more and more demanding, which requires the addition of lubricants to the coating. Lubricants can reduce the friction coefficient of the coating, improve the rheology of the coating, and then improve the flatness of the coating and the gloss of the finished paper. However, in order to reduce production costs, paper mills continue to increase the solid content of the coating, while the maximum solid content of lubricants on the market can only reach 50%, which is difficult to meet market requirements: In addition, the lubrication performance of high-solid content coatings is greatly reduced, which requires more efficient lubricants to meet market requirements.

[0004] At present, there are three main types of lubricants used for coated paper types such as coated white board paper, coated paper, and light coated paper: one is calcium stearate lubricants; one is oxidized polyethylene wax lubricants; and the other is fatty acid polyoxyethylene ether lubricants. The main preparation method of the first type of lubricant is: sodium stearate is generated by reacting stearic acid with sodium hydroxide, and then sodium stearate reacts with calcium chloride at a very low concentration to generate calcium stearate, and then it is washed several times, centrifugally dried, and dried in a drying oven to obtain relatively pure calcium stearate, and finally water and an emulsifier are added to the calcium stearate and emulsified by a high-pressure homogenizer. The whole process is complicated and cumbersome, the amount of waste water generated in the production is large, the product loss is large, and when the solid content of the lubricant is higher than 50%, the viscosity of the lubricant is very large and cannot meet the use requirements; the second type of lubricant contains waxy substances, which have a certain effect on the ink absorption of paper and cannot meet the production requirements of modern high-speed coated paper machines: although the solid content of the third type of lubricant can reach about 55%, the cost is too high, which adds a great cost burden to the production enterprise, and the rheological properties of the lubricant are poor, and paper defects such as streaks, orange peels, and rolling marks are prone to occur during the coating process.

[0005] In summary, it is necessary to provide a new type of high-efficiency lubricant for papermaking to reduce or avoid the occurrence of streaks, orange peels, rolling marks, etc. during application. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a water-based lubricant for papermaking coating and its application. The lubricant provided by the present invention solves the problem of poor fluidity in the coating coating process, reduces or even avoids streaks, orange peels, and rolling marks in the coating process; and shrinkage cavities, pinhole sagging, and the like in the drying process.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing an aqueous lubricant for paper coating. The aqueous lubricant for paper coating comprises, by weight: 13 to 18 parts of an aqueous oxidized polyethylene copolymer, 3 to 8 parts of a surfactant, 5 to 7 parts of a bactericide, 10 to 12 parts of an initiator and 100 parts of water.

[0009] Exemplarily, the weight proportion of the aqueous oxidized polyethylene copolymer in the aqueous lubricant for paper coating is 13 to 18 parts, for example, 13 parts, 13.5 parts, 14 parts, 14.5 parts, 15 parts, 15.5 parts, 16 parts, 16.5 parts, 17 parts, 17.5 parts or 18 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0010] In the present invention, the water-based oxidized polyethylene copolymer is the main component of the water-based lubricant for papermaking coating, is easily soluble in water, and is an anionic organic matter; in the water-based lubricant for papermaking coating, if the content of the water-based oxidized polyethylene copolymer is too high, the pH value of the water-soluble lubricant will be too large. When the pH is greater than 9.5, the viscosity of the water-soluble lubricant increases, and when it is mixed with papermaking coating for coating, streaking paper disease and the like will occur; if the content of the water-based oxidized polyethylene copolymer is too low, the water-based lubricant will fail to play a lubricating role.

[0011] The weight proportion of the surfactant is 3 to 8 parts, for example, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts or 8 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0012] The surfactant includes hydrogen peroxide and / or caustic soda.

[0013] The weight proportion of the bactericide is 5 to 7 parts, for example, 5 parts, 5.5 parts, 6 parts, 6.5 parts or 7 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0014] In the present invention, there is no specific limitation on the type of the bactericide, as long as it can sterilize the aqueous lubricant and does not affect the function of the aqueous lubricant.

[0015] The weight proportion of the initiator is 10 to 12 parts, for example, 10 parts, 10.5 parts, 11 parts, 11.5 parts or 12 parts, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0016] The initiator includes dimethyl azobisisobutyrate and / or azobisisobutyramidine hydrochloride.

[0017] As a preferred technical solution of the present invention, the solid content of the aqueous lubricant for paper coating is 23 to 28 wt%, for example, it can be 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt% or 28 wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Preferably, the viscosity of the aqueous lubricant for papermaking coating is ≤300cps, for example, it can be 300cps, 280cps, 260cps, 240cps, 220cps or 200cps, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the pH value of the aqueous lubricant for papermaking coating is 7-10, for example, 7, 7.3, 7.6, 7.9, 8.2, 8.5, 8.8, 9.1, 9.4, 9.7 or 10, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] In the present invention, the aqueous lubricant can improve the fluidity and leveling of the coating, make the paper coating smooth and uniform, improve the smoothness of the paper surface, reduce the cracking of the dry coating, reduce the hair loss and powder loss during the printing process, and is conducive to the preparation of high solid content coatings;

[0021] In addition, the solid content of the aqueous lubricant of the present invention is 23-28wt%. If the solid content is lower than 23wt%, the lubricating effect of the aqueous lubricant will be reduced, and the coating lubrication effect cannot be achieved; if the solid content is too high, the cost and pH value will increase. When the pH value is greater than 9.5, the aqueous lubricant affects the dispersibility of the papermaking coating, resulting in the coating being unable to disperse, thereby affecting the use effect.

[0022] It is worth noting that the water-based oxidized polyethylene copolymer of the present invention is acidic or neutral, but after being mixed with water, surfactants, bactericides and initiators, the resulting water-based lubricant is alkaline. The reason is that after adding surfactants and initiators, OH - The reaction is promoted so that the lubricant is alkaline.

[0023] As a preferred technical solution of the present invention, the preparation method of the aqueous oxidized polyethylene copolymer comprises:

[0024] (1) mixing ethylene oxide and polyethylene oxide, and then sequentially performing a mixing reaction and standing to obtain a reaction solution;

[0025] (2) mixing the amide and the reaction solution obtained in step (1), and subjecting the mixture to a modification reaction to obtain the water-based oxidized polyethylene copolymer.

[0026] As a preferred technical solution of the present invention, the mass ratio of ethylene oxide, amide and polyethylene oxide is 1.8-2.2:1:2.8-3.2, for example, it can be 1.8:1:2.8, 1.8:1:3.2, 2:1:3, 2:1:2.9, 2.2:1:3, 2.2:1:3.2 or 1.9:1:3.1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] As a preferred technical solution of the present invention, the temperature of the mixed reaction in step (1) is 60-70°C, for example, it can be 60°C, 62°C, 64°C, 66°C, 68°C or 70°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the stirring rate of the mixing reaction in step (1) is 800-1200 r / min, for example, it can be 800 r / min, 900 r / min, 1000 r / min, 1100 r / min or 1200 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the mixing reaction time in step (1) is 8 to 12 minutes, for example, 8 minutes, 9 minutes, 10 minutes, 11 minutes or 12 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the standing time in step (1) is 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] As a preferred technical solution of the present invention, the temperature of the modification reaction in step (2) is 25-30°C, for example, it can be 25°C, 26°C, 27°C, 28°C, 29°C or 30°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the modification reaction time in step (2) is 30 to 50 min, for example, 30 min, 34 min, 38 min, 42 min, 46 min or 50 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the stirring rate of the modification reaction in step (2) is 700-800 r / min, for example, it can be 700 r / min, 720 r / min, 740 r / min, 760 r / min, 780 r / min or 800 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the pH value of the modification reaction in step (2) is 5 to 7, for example, 5, 5.2, 5.4, 5.6, 5.8, 6, 6.2, 6.4, 6.6, 6.8 or 7, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] In the present invention, the water-based oxidized polyethylene copolymer prepared by amide modification has the characteristics of low temperature resistance and can be stored at a temperature of 0 to 5°C without affecting the use effect; the temperature during the modification reaction is 25 to 30°C. When the temperature is too high, the chemical properties of the modifier (amide) will be destroyed, causing it to lose its modification effect; the pH value of the modification reaction is 5 to 7. If the pH value is too high, the hydroxide content will be too high, which will prevent the decomposition and modification of the amide; if the pH value is too low, the modifier will react with the acid first and then be modified, and the effect will be weakened.

[0036] It is worth noting that the modification environment of the modification reaction in step (2) of the present invention can be neutral or acidic. When the modification environment is acidic, the pH value of the modification environment can be adjusted by adding an acid-base regulator to the mixed reaction in step (1).

[0037] In a second aspect, the present invention provides an application of the aqueous lubricant for paper coating provided in the first aspect in paper coating, wherein the application comprises the following steps:

[0038] (a) mixing alkali liquor, papermaking coating and the aqueous lubricant for papermaking coating to obtain a coating solution;

[0039] (b) Roll-coating the coating solution obtained in step (a) on at least one side of the paper layer to obtain a paper layer with a coating layer.

[0040] As a preferred technical solution of the present invention, the addition amount of the aqueous lubricant for paper coating in step (a) is 0.05-0.15% of the mass of the paper coating, for example, it can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14% or 0.15%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, the pH value of the coating solution in step (a) is 8.8-9.2, for example, 8.8, 8.9, 9.0, 9.1 or 9.2, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] Preferably, the alkali solution in step (a) comprises sodium hydroxide and / or calcium hydroxide.

[0043] As a preferred technical solution of the present invention, the roller coating in step (b) includes primer coating, mid-coating and top-coating performed sequentially.

[0044] Preferably, the roller coating temperature in step (b) is 58-65°C, for example, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C or 65°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] Preferably, the interval between two adjacent roller coatings is 3 to 5 seconds, for example, 3 seconds, 3.4 seconds, 3.8 seconds, 4.2 seconds, 4.6 seconds or 5 seconds, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] As a preferred technical solution of the present invention, the thickness of the coating obtained by each roller coating is 40-60 μm, for example, it can be 40 μm, 42 μm, 44 μm, 46 μm, 48 μm, 50 μm, 52 μm, 54 μm, 56 μm, 58 μm or 60 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0048] The system refers to an equipment system, a device system or a production device.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] (1) The aqueous lubricant provided by the present invention can effectively improve the fluidity and leveling properties of papermaking coatings, making the coating on the paper surface smooth and uniform, thereby improving the smoothness of the paper surface and reducing cracking of the coating and hair loss and powder loss during printing;

[0051] (2) The aqueous lubricant provided by the present invention has a relatively high solid content, so that the papermaking coating used in combination with the aqueous lubricant also has a relatively high solid content;

[0052] (3) The aqueous lubricant provided by the present invention has excellent stability and can be used normally within the temperature range of 20 to 200° C. without affecting its lubrication effect;

[0053] (4) The aqueous lubricant provided by the present invention is low in cost and is conducive to industrial application. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0055] Example 1

[0056] The present embodiment provides an aqueous lubricant for papermaking coating, which comprises, by weight, 15 parts of an aqueous oxidized polyethylene copolymer, 5 parts of a surfactant, 6 parts of a bactericide, 11 parts of an initiator, and 100 parts of water.

[0057] The water-based lubricant for papermaking coating has a solid content of 25 wt %, a viscosity of 280 cps, and a pH value of 8.5;

[0058] The preparation method of the water-based oxidized polyethylene copolymer comprises the following steps:

[0059] (1) mixing ethylene oxide and oxidized polyethylene, and then performing a mixing reaction at a temperature of 65° C. and a stirring rate of 1000 r / min for 10 minutes, and standing for 8 minutes to obtain a reaction solution; (2) mixing amide and the reaction solution obtained in step (1), and performing a modification reaction at a temperature of 25° C., a stirring rate of 750 r / min and a pH value of 6 for 40 minutes to obtain the water-based oxidized polyethylene copolymer;

[0060] Wherein, the mass ratio of ethylene oxide, amide and polyethylene oxide is 2:1:3.

[0061] Example 2

[0062] The present embodiment provides an aqueous lubricant for papermaking coating, which comprises, by weight, 13 parts of an aqueous oxidized polyethylene copolymer, 3 parts of a surfactant, 5 parts of a bactericide, 10 parts of an initiator, and 100 parts of water.

[0063] The water-based lubricant for papermaking coating has a solid content of 23 wt %, a viscosity of 240 cps, and a pH value of 10;

[0064] The preparation method of the water-based oxidized polyethylene copolymer comprises the following steps:

[0065] (1) mixing ethylene oxide and polyethylene oxide, and then performing a mixing reaction at a temperature of 60° C. and a stirring rate of 1200 r / min for 12 minutes, and standing for 10 minutes to obtain a reaction solution; (2) mixing amide and the reaction solution obtained in step (1), and performing a modification reaction at a temperature of 30° C., a stirring rate of 700 r / min and a pH value of 7 for 50 minutes to obtain the water-based polyethylene oxide copolymer;

[0066] Wherein, the mass ratio of ethylene oxide, amide and polyethylene oxide is 1.8:1:2.8.

[0067] Example 3

[0068] The present embodiment provides an aqueous lubricant for papermaking coating, which comprises, by weight, 18 parts of an aqueous oxidized polyethylene copolymer, 8 parts of a surfactant, 7 parts of a bactericide, 12 parts of an initiator, and 100 parts of water.

[0069] The water-based lubricant for papermaking coating has a solid content of 28 wt %, a viscosity of 300 cps, and a pH value of 7;

[0070] The preparation method of the water-based oxidized polyethylene copolymer comprises the following steps:

[0071] (1) mixing ethylene oxide and polyethylene oxide, and then performing a mixing reaction at a temperature of 70° C. and a stirring rate of 800 r / min for 8 minutes, and standing for 5 to 10 minutes to obtain a reaction solution; (2) mixing amide and the reaction solution obtained in step (1), and performing a modification reaction at a temperature of 25° C., a stirring rate of 800 r / min and a pH value of 5 for 30 minutes to obtain the water-based polyethylene oxide copolymer;

[0072] Wherein, the mass ratio of ethylene oxide, amide and polyethylene oxide is 2.2:1:3.2.

[0073] Example 4

[0074] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0075] In this example, the temperature of the modification reaction in step (2) is adjusted to 40°C.

[0076] The aqueous lubricant provided in this embodiment has a solid content of 25 wt %, a viscosity of 260 cps, and a pH value of 8.5.

[0077] The modification reaction temperature in this embodiment is too high, which causes the structure of the modifier amide to be destroyed, thereby losing the modification ability.

[0078] Example 5

[0079] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0080] In this example, the temperature of the modification reaction in step (2) is adjusted to 20°C.

[0081] The aqueous lubricant provided in this embodiment has a solid content of 25 wt %, a viscosity of 200 cps, and a pH value of 6.5.

[0082] Example 6

[0083] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0084] In this embodiment, the pH value of the modification reaction in step (2) is adjusted to 3.

[0085] The aqueous lubricant provided in this embodiment has a solid content of 25 wt %, a viscosity of 198 cps, and a pH value of 6.

[0086] Example 7

[0087] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0088] In this embodiment, the pH value of the modification reaction in step (2) is adjusted to 8.

[0089] The aqueous lubricant provided in this embodiment has a solid content of 25.5 wt %, a viscosity of 230 cps, and a pH value of 8.4.

[0090] Example 8

[0091] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0092] In this embodiment, the mass ratio of ethylene oxide, amide and polyethylene oxide is adjusted to 1.5:2:2.

[0093] The aqueous lubricant provided in this embodiment has a solid content of 24.5 wt %, a viscosity of 240 cps, and a pH value of 8.

[0094] Example 9

[0095] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0096] In this embodiment, the mass ratio of ethylene oxide, amide and polyethylene oxide is adjusted to 2.5:2:3.6.

[0097] The aqueous lubricant provided in this embodiment has a solid content of 25 wt %, a viscosity of 290 cps, and a pH value of 9.

[0098] Comparative Example 1

[0099] This embodiment provides an aqueous lubricant for papermaking coating, and the aqueous lubricant for papermaking coating is different from that of embodiment 1 only in that:

[0100] In this comparative example, the modification reaction described in step (2) is omitted, that is, the water-based oxidized polyethylene copolymer in the water-based lubricant for papermaking coating is not modified.

[0101] The aqueous lubricant provided in this comparative example has a solid content of 26 wt %, a viscosity of 270 cps, and a pH value of 8.8.

[0102] Application Example 1

[0103] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating, and the application comprises the following steps:

[0104] (a) mixing an alkali solution, a papermaking coating and an aqueous lubricant for papermaking coating to obtain a coating solution having a pH value of 9;

[0105] Wherein, the amount of water-based lubricant added for paper coating is 0.1% of the mass of the paper coating;

[0106] (b) applying the coating solution obtained in step (a) to at least one side of the paper layer with a roller to obtain a paper layer with a coating;

[0107] The roller coating includes primer coating, intermediate coating and top coating in sequence; the temperature of the roller coating is 60° C., the interval between two adjacent roller coatings is 4 seconds; the thickness of the coating obtained by each roller coating is 50 μm.

[0108] Application Example 2

[0109] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating, and the application comprises the following steps:

[0110] (a) mixing an alkali solution, a papermaking coating and an aqueous lubricant for papermaking coating to obtain a coating solution having a pH value of 8.8;

[0111] Wherein, the amount of water-based lubricant added for paper coating is 0.05% of the mass of the paper coating;

[0112] (b) applying the coating solution obtained in step (a) to at least one side of the paper layer with a roller to obtain a paper layer with a coating;

[0113] The roller coating includes primer coating, intermediate coating and top coating in sequence; the temperature of the roller coating is 58° C., and the interval between two adjacent roller coatings is 5s; the thickness of the coating obtained by each roller coating is 60 μm.

[0114] Application Example 3

[0115] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating, and the application comprises the following steps:

[0116] (a) mixing an alkali solution, a papermaking coating and an aqueous lubricant for papermaking coating to obtain a coating solution having a pH value of 9.2;

[0117] Wherein, the amount of water-based lubricant added for paper coating is 0.15% of the mass of the paper coating;

[0118] (b) applying the coating solution obtained in step (a) to at least one side of the paper layer with a roller to obtain a paper layer with a coating;

[0119] The roller coating includes primer coating, intermediate coating and top coating in sequence; the temperature of the roller coating is 65° C., the interval between two adjacent roller coatings is 3 seconds; the thickness of the coating obtained by each roller coating is 40 μm.

[0120] Application Example 4-9

[0121] An application of the aqueous lubricant for paper coating provided by Examples 4-9 in paper coating, wherein the operation steps of the application are the same as those of Application Example 1.

[0122] Application Example 10

[0123] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating. The difference between the application and Application Example 1 is that:

[0124] In this application example, the amount of the aqueous lubricant added for paper coating in step (a) is adjusted to 2% of the mass of the paper coating.

[0125] Application Example 11

[0126] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating. The difference between the application and Application Example 1 is that:

[0127] In this application example, the amount of the aqueous lubricant added for paper coating in step (a) is adjusted to 0% of the mass of the paper coating.

[0128] Application Example 12

[0129] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating. The difference between the application and Application Example 1 is that:

[0130] In this application example, the pH value of the coating solution in step (a) is adjusted to 10.

[0131] Application Example 13

[0132] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating. The difference between the application and Application Example 1 is that:

[0133] In this application example, the pH value of the coating solution in step (a) is adjusted to 7.

[0134] Application Example 13

[0135] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating. The difference between the application and Application Example 1 is that:

[0136] In this application example, the thickness of the coating obtained by each roller coating in step (b) is adjusted to 30 μm.

[0137] Application Example 14

[0138] This application example provides an application of the aqueous lubricant for paper coating provided in Example 1 in paper coating. The difference between the application and Application Example 1 is that:

[0139] In this application example, the thickness of the coating obtained by each roller coating in step (b) is adjusted to 70 μm.

[0140] Comparative application example 1

[0141] This comparative application example provides an application of the aqueous lubricant for paper coating provided in Comparative Example 1 in paper coating, and the operation steps of the application are the same as those of Application Example 1.

[0142] Coating performance test:

[0143] The coating performance test of the coated paper provided in the above application examples and comparative application examples was carried out using the national standard method, and the results are shown in Table 1:

[0144] Among them, the paper used in the coating process is: gray-based white board paper.

[0145] Table 1

[0146]

[0147]

[0148] According to Table 1, we can know the following points:

[0149] (1) Comprehensive analysis of application examples 1-3 shows that the whiteness of the paper layer with coating obtained by using the lubricant provided by the present invention is 78.4-78.6%, the smoothness is 220-240s, the roughness is 1.00-1.04μm, and the gloss is 51-52GU; this shows that the lubricant provided by the present invention can improve the fluidity and leveling of the coating, make the paper surface coating smooth and uniform, and improve the smoothness of the paper surface;

[0150] (2) Comprehensive analysis of Application Example 1, Application Examples 4-7 and Comparative Application Example 1 shows that adjustment of the preparation parameters of the water-based oxidized polyethylene copolymer in the water-based lubricant will affect the performance of the water-based oxidized polyethylene copolymer, and thus affect the effect of the lubricant;

[0151] Among them, if the temperature of the modification reaction is too high or too low (such as application example 4-5) or the pH value of the modification reaction is too high or too low, the whiteness, glossiness and smoothness of the coated paper will decrease, and the roughness will also increase;

[0152] If the modification process is omitted (such as in Comparative Example 1), the smoothness and glossiness will be greatly reduced, and the roughness will increase;

[0153] (3) Comprehensive analysis of Application Examples 1 and 10-14 shows that the selection of process parameters during coating will also affect the effect of the lubricant, that is, the whiteness of the paper layer after coating and other paper indicators;

[0154] Among them, during the coating process, if the amount of water-based lubricant added is too high or too low (such as application examples 10-11), the smoothness will decrease and the roughness will increase;

[0155] During the coating process, if the pH value of the coating solution is too high (such as in Application Example 12), it will result in high roughness, low whiteness and low gloss; if the coating solution is neutral (such as in Application Example 13), it will result in decreased gloss and smoothness, and increased roughness;

[0156] In summary, the lubricant provided by the present invention solves the problem of poor fluidity during coating application, reduces or even avoids streaks, orange peels, and rolling marks during the coating process, and craters, pinholes, and sagging that occur during the drying process.

[0157] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based lubricant for papermaking coating, characterized in that: The aqueous lubricant for papermaking coating comprises, by weight: 13 to 18 parts of aqueous oxidized polyethylene copolymer, 3 to 8 parts of surfactant, 5 to 7 parts of bactericide, 10 to 12 parts of initiator and 100 parts of water.

2. The aqueous lubricant for paper coating according to claim 1, characterized in that: The solid content of the water-based lubricant for papermaking coating is 23-28 wt %; Preferably, the viscosity of the aqueous lubricant for papermaking coating is ≤300cps; Preferably, the pH value of the aqueous lubricant for papermaking coating is 7-10.

3. The aqueous lubricant for papermaking coating according to claim 1 or 2, characterized in that: The preparation method of the aqueous oxidized polyethylene copolymer comprises the following steps: (1) mixing ethylene oxide and polyethylene oxide, and then sequentially performing a mixing reaction and standing to obtain a reaction solution; (2) mixing the amide and the reaction solution obtained in step (1), and subjecting the mixture to a modification reaction to obtain the water-based oxidized polyethylene copolymer.

4. The aqueous lubricant for papermaking coating according to claim 3, characterized in that: The mass ratio of the ethylene oxide, amide and polyethylene oxide is 1.8-2.2:1:2.8-3.

2.

5. The aqueous lubricant for papermaking coating according to claim 3, characterized in that: The temperature of the mixed reaction in step (1) is 60-70° C. Preferably, the stirring rate of the mixing reaction in step (1) is 800 to 1200 r / min; Preferably, the mixing reaction time in step (1) is 8 to 12 minutes; Preferably, the standing time in step (1) is 5 to 10 minutes.

6. The aqueous lubricant for papermaking coating according to claim 3, characterized in that: The temperature of the modification reaction in step (2) is 25-30° C. Preferably, the modification reaction time in step (2) is 30 to 50 minutes; Preferably, the stirring rate of the modification reaction in step (2) is 700-800 r / min; Preferably, the pH value of the modification reaction in step (2) is 5-7.

7. Use of the aqueous lubricant for paper coating as claimed in any one of claims 1 to 6 in paper coating, characterized in that: The application comprises the following steps: (a) mixing alkali liquor, papermaking coating and the aqueous lubricant for papermaking coating to obtain a coating solution; (b) Roll-coating the coating solution obtained in step (a) on at least one side of the paper layer to obtain a paper layer with a coating layer.

8. The use according to claim 7, characterized in that: The amount of the aqueous lubricant added in step (a) for paper coating is 0.05-0.15% of the mass of the paper coating; Preferably, the pH value of the coating solution in step (a) is 8.8-9.

2.

9. The use according to claim 7 or 8, characterized in that: The roller coating in step (b) includes primer coating, mid-coating and top-coating performed sequentially; Preferably, the temperature of the roller coating in step (b) is 58-65°C; Preferably, the interval between two adjacent roller coatings is 3 to 5 seconds.

10. The use according to any one of claims 7 to 9, characterized in that: The thickness of the coating obtained by each roller coating is 40-60 μm.

Citation Information

Patent Citations

  • Lubricant for papermaking and preparation method thereof

    CN106245429A

  • Multifunctional coating lubricant as well as preparation method and application thereof

    CN112574367A

  • Lubricant additives for paper coating compositions

    US5527383A