Preparation method of two-dimensional rhombic-phase ZnIn2S4 nanosheet array photo-anode, layer thickness regulation and control method and photoelectric detection application of two-dimensional rhombic-phase ZnIn2S4 nanosheet array photo-anode

By regulating the concentration of thiourea on the conductive substrate FTO, the ZnIn2S4 nanosheet array with different thicknesses is grown by hydrothermal method, the problem of insufficient application of ZnIn2S4 in the field of photoelectric detection is solved, and the two-way regulation and application expansion of photoelectric detection performance is realized, and the improvement of the optimization performance is improved. The performance of the photodetector.

CN118980724AActive Publication Date: 2024-11-19HANGZHOU DIANZI UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411124346.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

ZnIn2S4 is insufficiently used in the field of photoelectric detection, especially the layer thickness regulation strategy is not fully explored, which limits the optimization and application potential of its photoelectric detection performance.

Method used

By regulating the concentration of thiourea, ZnIn2S4 nanosheet arrays of different layers of thickness were grown in situ on the conductive substrate FTO, a ZnIn2S4 PEC self-powered photodetector was prepared, which realized the bidirectional regulation of photodetection performance and broadened the spectrum. Respond and optimize UV ​​detection performance.

Benefits of technology

The wide spectrum detection of multi-layer ZnIn2S4 and the ultraviolet detection performance optimization of single-layer ZnIn2S4 are achieved, which improves the photoresponse and detection rate of the photodetector, and has ultra-high photoresponse and detection rate without external bias.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980724A_ABST
    Figure CN118980724A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a two-dimensional rhombic-phase ZnIn2S4 nanosheet array photo-anode, a layer thickness regulation and control method and photoelectric detection application of the two-dimensional rhombic-phase ZnIn2S4 nanosheet array photo-anode. On a clean conductive substrate FTO (Fluorine-doped Tin Oxide), an aqueous solution containing ZnCl2, InCl3. 4H2O and CH4N2S is used as a precursor solution, and the ZnIn2S4 nanosheet array photo-anode is directly prepared in situ through a one-step simple hydrothermal method. The ZnIn2S4-based PEC type self-powered photoelectric detector comprises an electrolyte, a reference electrode, a working electrode and a counter electrode, wherein the working electrode is a ZnIn2S4 nanosheet array photo-anode. The invention develops a confinement growth method based on thiourea concentration regulation and control to bidirectionally regulate and control layer number stacking of ZnIn2S4 atomic layers, so that a ZnIn2S4PEC type self-powered photoelectric detector is prepared based on ZnIn2S4 with different layer numbers. According to the tunable photoelectric characteristic of ZnIn2S4 with different layer numbers, wide-spectrum photoelectric detection and ultraviolet photoelectric detection are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photoelectric detection, and specifically relates to a preparation method of a two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode, a layer thickness control method and a photoelectric detection application. Background Art

[0002] Two-dimensional (2D) spatial confinement endows layered van-der-Waals materials with unique electronic and optoelectronic properties, which have attracted great research attention in the fields of information devices and energy conversion. One of the most fascinating properties of 2D materials is the layer-number dependence of the electronic structure caused by the interlayer coupling effect, which provides an opportunity to easily tune their band structure and optoelectronic properties for multifunctional applications. In-depth exploration of the relationship between the number of layers and the electronic structure will enable precise control of the photogenerated carrier dynamics, including the generation, separation and interface transfer behavior of photogenerated carriers, thereby optimizing and expanding their optoelectronic applications.

[0003] As a typical member of the emerging two-dimensional ternary metal chalcogenides (TMCs), ZnIn2S4 with layered hexagonal and rhombohedral crystal phase structures has superior optoelectronic properties, high conduction band bottom position, rich tunability and more ideal chemical stability compared with other two-dimensional materials (such as BP and TMDs), and therefore has broad application prospects as a semiconductor photocatalyst in the field of solar energy conversion. In addition, the two-dimensional morphology not only gives ZnIn2S4 a large specific surface area, but also shortens the diffusion distance of carriers to the surface, which is beneficial to heterogeneous interface coupling and interfacial carrier transport with other semiconductors or electrolytes. Although various strategies including doping with heteroatoms and incorporating vacancies have been adopted to adjust its electronic structure to further optimize photocarrier dynamics and improve photon utilization, the fascinating strategy of controlling layer thickness, which is only allowed by two-dimensional materials, has remained almost unexplored in ZnIn2S4.

[0004] Although ZnIn2S4 has excellent optoelectronic properties, fast response and low dark current as a two-dimensional material, its application in the field of photodetection is almost blank. In recent years, photoelectrochemical (PEC) type photodetectors (PDs) with simple device structure have become ideal candidate materials for realizing self-powered functions, which is in line with the development trend of low energy consumption. These advantages of ZnIn2S4 show great potential in PEC type PDs. The more common application scenarios of PEC type photodetectors are highly integrated broadband light detection and deep ultraviolet light detection for underwater optical communications. The layered band structure of ZnIn2S4 provides an opportunity to integrate these two applications into one semiconductor. Summary of the invention

[0005] In view of the shortcomings of ZnIn2S4 in the field of photoelectric detection, the present invention aims to provide a two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode preparation, layer thickness control method and photoelectric detection application. Through a one-step simple hydrothermal method to control the concentration of thiourea, ZnIn2S4 nanosheet arrays with different layer thicknesses are in situ grown on a conductive substrate FTO, thereby preparing a ZnIn2S4 PEC type self-powered photodetector based on ZnIn2S4 with different layer thicknesses, and realizing the two-way control of the photoelectric detection performance of the ZnIn2S4 PEC type self-powered photodetector. On the one hand, multilayer ZnIn2S4 achieves the effect of wide spectrum detection by broadening the wavelength band and improving the light response; on the other hand, the ultraviolet detection performance of the single-layer ZnIn2S4 is optimized.

[0006] The present invention provides a method for preparing a two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode, comprising the following steps:

[0007] (1) Obtain clean conductive glass FTO;

[0008] (2) mixing the following raw materials according to a preset ratio: ZnCl2, InCl3·4H2O and CH4N2S, and dissolving them in water to obtain a precursor solution;

[0009] (3) subjecting the conductive glass FTO conductive surface described in step (1) to plasma surface treatment;

[0010] Within the effective time after the plasma surface treatment, two FTO sheets are placed in a reaction container in a "V" shape with the conductive surface facing downward, and the precursor solution prepared in step (2) is added to perform a hydrothermal reaction, thereby obtaining a two-dimensional rhombus phase ZnIn2S4 nanosheet array on the conductive surface of the conductive glass FTO;

[0011] Conductive glass FTO and the conductive surface of the conductive glass FTO are used together to obtain a two-dimensional rhombus phase ZnIn2S4 nanosheet array, which are used as a photoanode for making a working electrode of a PEC type self-powered photodetector; the prepared two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode includes: conductive glass FTO and a two-dimensional rhombus phase ZnIn2S4 nanosheet array in-situ grown on the conductive surface of the conductive glass FTO; the two-dimensional rhombus phase ZnIn2S4 nanosheet array is composed of stacked two-dimensional rhombus phase ZnIn2S4 nanosheets; the layer thickness of the two-dimensional rhombus phase ZnIn2S4 nanosheet is 4nm to 44.8nm.

[0012] Layered rhombohedral phase-structured ZnIn2S4 has shown great promise as a semiconductor photocatalyst in solar energy conversion in recent years due to its superior optoelectronic properties, high CBM sites, rich tunability, and more desirable chemical stability than other 2D materials (e.g., BP, TMDs). To further optimize photocarrier dynamics and improve photon utilization, various strategies such as heteroatom doping and vacancy incorporation have been adopted to tune its electronic structure, but controlling layer thickness, a fascinating strategy that is only allowed in 2D materials, has hardly been fully explored.

[0013] Preferably, in step (2), the setting of the preset ratio comprises the following steps:

[0014] Obtaining the wavelength range of the detection target of the PEC type self-powered photoelectric detector; setting the preset ratio according to the wavelength range of the detection target;

[0015] When the wavelength range of the detection target is 355-765 nm, the preset molar ratio of ZnCl2, InCl3·4H2O and CH4N2S is: 1:2:4;

[0016] When the wavelength range of the detection target is 254-355 nm, the preset molar ratio of ZnCl2, InCl3·4H2O and CH4N2S is 1:2:16.

[0017] Preferably, in step (3), the reaction container is a polytetrafluoroethylene liner; the hydrothermal reaction specifically includes: placing the polytetrafluoroethylene liner in a high-pressure reactor and performing a hydrothermal reaction at a temperature of 170°C for 12 hours; the plasma treatment specifically includes the following steps: treating in a plasma cleaner with a power of 60W and a time of 120s; the effective time refers to the time after the plasma treatment when the surface of the conductive glass FTO has energy within a certain period of time, which can promote the growth of the compound on the FTO surface, and the effective time is 10 minutes.

[0018] The present invention also provides a photoelectric detection application of a two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode, comprising the following steps:

[0019] Constructing a PEC type self-powered photodetector, using the two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode as a working electrode of the PEC type self-powered photodetector;

[0020] The PEC type self-powered photoelectric detector also includes an electrochemical workstation, an electrolyte tank, a reference electrode and a counter electrode; an electrolyte is provided in the electrolyte tank, and the reference electrode, the working electrode and the counter electrode are suspended in the electrolyte tank, all in contact with the electrolyte, and none of them touch the bottom of the electrolyte tank;

[0021] The working electrode is connected to the positive pole of the power supply of the electrochemical workstation, the counter electrode is connected to the negative pole of the power supply of the electrochemical workstation, and the reference electrode is connected to the reference potentiometer of the electrochemical workstation.

[0022] Preferably, the electrolyte in the electrolyte solution is 0.5M Na2SO4 and 0.2M Na2SO3; the reference electrode is an Ag / AgCl electrode; and the counter electrode is a Pt electrode.

[0023] The present invention also provides a method for controlling the layer thickness of a two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode, wherein the two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode is prepared using the method for preparing the two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode, and the layer thickness of the two-dimensional rhombus phase ZnIn2S4 nanosheet obtained on the conductive surface of conductive glass FTO in step (3) is adjusted by adjusting the preset ratio in step (2); when the preset molar ratio of ZnCl2, InCl3·4H2O and CH4N2S is 1:2:4, the layer thickness of the two-dimensional rhombus phase ZnIn2S4 nanosheet is 44.8nm; when the preset molar ratio of ZnCl2, InCl3·4H2O and CH4N2S is 1:2:8, the layer thickness of the two-dimensional rhombus phase ZnIn2S4 nanosheet is 18.6nm; when the preset molar ratio of ZnCl2, InCl3·4H2O and CH4N2S is 1:2:12, the layer thickness of the two-dimensional rhombus phase ZnIn2S4 nanosheet is 11.5nm; when the preset molar ratio of ZnCl2, InCl3·4H2O and CH4N2S is 1:2:16, the layer thickness of the two-dimensional rhombus phase ZnIn2S4 nanosheet is 4nm.

[0024] Therefore, the present invention is based on regulating the stacking of two-dimensional rhombohedral phase ZnIn2S4 atomic layers to adjust its band structure and photoelectric properties, and further produces a wide spectrum and ultraviolet PEC type self-powered photodetector based on ZnIn2S4. The photodetector combines the excellent photoelectric properties, self-powered properties, fast response and low dark current of ZnIn2S4 itself, as well as the regulation of the band structure and photoelectric properties, so that the photodetector has ultra-high light responsiveness and detection rate without the need for external bias. In addition, the two applications are integrated into a semiconductor ZnIn2S4, further expanding the application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the specific implementation of the present invention or the technical solutions in the prior art, the following will briefly introduce the drawings required for the specific implementation or the prior art description. Some specific embodiments of the present invention will be described in detail in an exemplary but not restrictive manner with reference to the drawings. The same reference numerals in the drawings indicate the same or similar components or parts. Those skilled in the art should understand that these drawings are not necessarily drawn to scale. In the drawings:

[0026] Figure 1 a, b, c, d are scanning electron microscope images of ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention, respectively. All prepared photoanodes are high-quality, large-area, two-dimensional nanosheet structures vertically distributed on the FTO surface. As the concentration of thiourea increases, the thickness of the ZnIn2S4 nanosheet gradually becomes thinner, evolving from the relatively straight thick nanosheet morphology of ZIS-4TU to the wrinkled, thin nanosheet of ZIS-16TU.

[0027] Figure 2 It is the X-ray diffraction pattern (XRD) of the ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3 and 4 of the present invention. After removing the characteristic diffraction peaks of the FTO substrate, the remaining diffraction peaks of ZIS-4TU, ZIS-8TU, ZIS-12TU and ZIS-16TU all correspond to the rhombic phase ZnIn2S4 (JCPDS card no.72-1445) ((009), (012), (104), (015), (018), (110), (119) and (202) are all characteristic diffraction peaks of the rhombic phase ZnIn2S4), and no other phases and impurity peaks are detected, indicating that the synthesized rhombic phase ZnIn2S4 has a high purity, and the sharp diffraction peaks indicate that the synthesized product has good crystallinity. In addition, from ZIS-4TU to ZIS-16TU, the (104) and (110) peak intensities of ZnIn2S4 gradually weaken due to the decrease of layer thickness and crystallinity.

[0028] Figure 3 a, b, c, d are the atomic force microscope (AFM) measurement results of the ZIS-4TU, ZIS-8TU, ZIS-12TU, and ZIS-16TU nanosheets prepared in Examples 1, 2, 3, and 4 of the present invention, respectively. The corresponding layer thicknesses of the ZIS-4TU, ZIS-8TU, ZIS-12TU, and ZIS-16TU nanosheets are 44.8 nm, 18.6 nm, 11.5 nm, and 4 nm, respectively.

[0029] Figure 4a in the figure is the UV-visible diffuse reflectance spectra of ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention, and the upper right inset is its band gap diagram. From ZIS-16TU, ZIS-12TU, ZIS-8TU to ZIS-4TU, the cutoff absorption edge gradually red-shifts. As the number of layers decreases, the optical band gap of ZnIn2S4 gradually increases from 2.39 eV to 2.77 eV, which should be attributed to the change in charge distribution caused by the interlayer van der Waals interaction.

[0030] Figure 4 b is the photoluminescence (PL) spectrum of ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention, with an excitation wavelength of 440 nm. From ZIS-16TU, ZIS-12TU, ZIS-8TU to ZIS-4TU, the PL peak gradually red shifts, further confirming that the direct band gap decreases with the increase of ZnIn2S4 atomic layer stacking.

[0031] Figure 5 The schematic diagram of the working mechanism of the PEC type photodetector based on ZnIn2S4 of the present invention includes a xenon lamp, an electrochemical workstation, an electrolyte tank, a working electrode, a counter electrode, and a reference electrode. F ) and the electrolyte redox potential (hydrogen evolution potential: H + / H2, oxygen generation potential: O2 / H2O), when the ZnIn2S4 working electrode and the electrolyte come into contact, a built-in electric field is formed at the interface. (CB: conduction band, VB: valence band) When light irradiates the working electrode, electron-hole pairs are generated. Then, the photoelectrons flow from ZnIn2S4 to FTO and enter the external circuit. The photogenerated holes are transmitted to the ZnIn2S4 / electrolyte interface and are OH - The photogenerated electrons reach the counter electrode (Pt) and react with the free radicals OH* to form OH -, so far the entire circuit reflux is completed and self-powered. ZnIn2S4 PEC photodetectors have the advantages of excellent photoelectric properties, fast response and low dark current compared to other materials. These advantages of ZnIn2S4 are used to realize the self-powered function of PEC photodetectors, which is in line with the development trend of low energy consumption. The more common application scenarios of PEC photodetectors are highly integrated broadband light detection and deep ultraviolet light detection for underwater optical communications. The layered band structure of ZnIn2S4 provides an opportunity to integrate these two applications into one semiconductor.

[0032] Figure 6 The photocurrent-to-amp characteristic curves of the ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention are shown in Table 1. All of these ZnIn2S4 nanosheets have high photocurrent density and excellent transient photoresponse at any bias voltage. With the increase in the number of layers and the decrease in the optical band gap, ZnIn2S4 can effectively utilize the long wavelength of sunlight. The maximum photocurrent of ZIS-4TU reaches 2.5 mA cm at 0.6 V vs. Ag / AgCl. -2 .

[0033] Figure 7 It is the response time curve of ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention under zero bias (0V (vs. Ag / AgCl)). The rise (decay) time is the response time of the photocurrent from 10% (90%) to 90% (10%). The rise time and decay time of these four ZnIn2S4 are all within tens of milliseconds. The rise / decay time of ZIS-4TU under 450nm illumination is 12.5ms / 5.3ms, the rise / decay time of ZIS-8TU under 450nm illumination is 14.9ms / 8.2ms, the rise / decay time of ZIS-12TU under 355nm illumination is 11.7ms / 6.7ms, and the rise / decay time of ZIS-16TU under 355nm illumination is 23.3ms / 10ms, showing fast light response under both visible light and ultraviolet light.

[0034] Figure 8 a and b are the transient light response behaviors of ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention at different wavelengths (254nm-650nm). Figure 8 0.0025 mA cm in a and b -2 , 0.1mA cm -2 , 0.05mA cm -2 , 0.001mA cm -2The scales on their left represent the scales of the layers they are on. All ZnIn2S4 photodetectors exhibit fast and stable transient photoresponses without external bias, showing their potential as self-powered photodetection devices. ZIS-4TU has the largest Iph in the full light range of 355-650nm, with the potential to further broaden the detection range, while ZIS-16TU exhibits the best photoresponse at 254nm, the visible light response at 450-650nm is successfully suppressed, and UV detection is optimized.

[0035] Figure 8 c and d are the responsivity and detectivity diagrams of ZnIn2S4 nanosheets with different precursor ratios prepared in Examples 1, 2, 3, and 4 of the present invention. ZIS-4TU has a high Rph (responsivity) from deep ultraviolet light to red light, and the maximum Rph reaches 90.29 mA W at 355 nm. -1 , demonstrating its potential in broadband light detection. However, ZIS-16TU only exhibits superior Rph in the UV band, reaching 90.13 mA W at 254 nm. -1 The best Rph of , showing its potential in the field of deep ultraviolet light detection. Thanks to the low dark current, all these ZnIn2S4 photodetectors show excellent specific detection capabilities at different wavelengths, up to 1.602×10 12 Jones.

[0036] Fig. 9 a and b are the transient light response behaviors of the ZIS-4TU photodetector prepared in Example 1 of the present invention at different light powers at wavelengths of 254-765nm. ZIS-4TU has excellent transient light response from 254nm deep ultraviolet to 765nm near infrared, and the response intensity increases continuously with the increase of power density, and the detection range can achieve a wide spectrum detection effect.

[0037] Fig.10 This is the transient light response behavior of the ZIS-16TU photodetector prepared in Example 4 of the present invention at different light powers at wavelengths of 254-650nm. The light response in the visible light band is successfully suppressed, while the light response in the ultraviolet band gradually increases with the increase of power density. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the present application clearer, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application.

[0039] Example 1 Preparation method of two-dimensional rhombohedral phase ZnIn2S4 nanosheet array photoanode

[0040] (1) The conductive glass FTO was ultrasonically cleaned with acetone, anhydrous ethanol, deionized water, and anhydrous ethanol for 15 minutes in sequence. After cleaning, the FTO was placed in the air to dry naturally.

[0041] (2) Weigh 34.8 mg ZnCl2, 148 mg InCl3·4H2O, and 76.9 mg CH4N2S powder into a beaker, add 18 mL (18 g) of deionized water, and stir with a magnetic stirrer to obtain a completely dissolved uniform precursor solution.

[0042] (3) Stick a high temperature resistant tape on one end of the conductive surface of the conductive glass FTO in step (1) to keep the conductive surface 1 cm 2 , keep 1cm 2 The purpose is to grow ZnIn2S4 only at 1cm 2 area, so that it is easy to calculate when doing performance testing. Then, with the conductive surface facing up, it is placed in a plasma cleaning machine for treatment. The plasma treatment power is 60W and the time is 120s. The purpose of the conductive surface facing up is to make it face the direction of ion emission. Within the effective time of 10 minutes, the two FTO sheets are placed in a V-shaped polytetrafluoroethylene liner with the conductive surface facing down, and the precursor solution prepared in step (2) is added. Place it in a forced air drying oven and heat it at 170°C for 12 hours. After the reaction is completed, take out the sample, and repeatedly rinse the surface impurities with deionized water and anhydrous ethanol. The obtained ZnIn2S4 photoanode sample is marked as ZIS-4TU.

[0043] (4) The ZIS-4TU nanosheets grown on the FTO surface were peeled off into ethanol and ultrasonicated in an ultrasonic cleaner for 30 min. The solution was then diluted with ethanol to a slightly yellow color. A small amount of the solution was dripped onto a silicon wafer and allowed to dry at room temperature. The thickness of a single ZIS-4TU nanosheet on the silicon wafer was measured using an atomic force microscope.

[0044] (5) The light absorption performance of the ZIS-4TU photoanode was characterized by using a UV-visible spectrophotometer. The ZIS-4TU photoanode grown on the FTO glass was directly embedded in a BaSO4 background white board to form a sample with a flat surface that was uniformly embedded in the BaSO4 background white board for testing. The test range was 200-800nm ​​and the spectral bandwidth was 5nm.

[0045] (6) The optical properties of the ZIS-4TU photoanode were characterized by photoluminescence spectroscopy. The ZIS-4TU photoanode grown on FTO glass was directly used for testing with an excitation wavelength of 440 nm and a test range of 460 nm-640 nm.

[0046] (7) The photoelectrochemical and photodetection performance of the ZIS-4TU photoanode was tested using a three-electrode system, with the ZIS-4TU photoanode as the working electrode, the Pt electrode as the counter electrode, the Ag / AgCl electrode as the reference electrode, and the electrolyte being a mixed aqueous solution of 0.5 M Na2SO4 and 0.2 M Na2SO3 (pH = 9.6). An AM 1.5G xenon lamp was used to simulate sunlight with an intensity of about 100 mW / cm 2 The potential test range of the linear voltammetric characteristic curve (LSV) is -0.8~0.6V (vs.Ag / AgCl), and the voltage scanning rate is 3mV / s. The photoelectric performance at different wavelengths uses a 254nm deep ultraviolet LED lamp and 355nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm and 765nm filters. The power size is divided into five energy levels: Ⅰ, Ⅱ, Ⅲ, Ⅳ, and Ⅴ. The cycle of the transient light response test is 10s (5s irradiation, 5s dark).

[0047] Example 2 Preparation method of two-dimensional rhombohedral phase ZnIn2S4 nanosheet array photoanode

[0048] (1) The conductive glass FTO was ultrasonically cleaned with acetone, anhydrous ethanol, deionized water, and anhydrous ethanol for 15 minutes in sequence. After cleaning, the FTO was placed in the air to dry naturally.

[0049] (2) Weigh 34.8 mg ZnCl2, 148 mg InCl3·4H2O and 153.8 mg CH4N2S powder into a beaker, add 18 mL (18 g) of deionized water, and stir with a magnetic stirrer to obtain a completely dissolved uniform precursor solution.

[0050] (3) Stick a high temperature resistant tape on one end of the conductive surface of the conductive glass FTO in step (1) to keep the conductive surface 1 cm 2 , then placed in a plasma cleaning machine with the conductive surface facing up, with a plasma treatment power of 60W for 120s. Within 10min of the effective time, two FTO sheets were placed in a polytetrafluoroethylene liner with the conductive surface facing down in a V shape, and the precursor solution prepared in step (2) was added. Placed in a blast drying oven and heated at 170°C for 12h. After the reaction was completed, the sample was taken out and the surface impurities were repeatedly washed with deionized water and anhydrous ethanol. The obtained ZnIn2S4 photoanode sample was marked as ZIS-8TU.

[0051] (4) The ZIS-8TU nanosheets grown on the FTO surface were peeled off into ethanol and ultrasonicated in an ultrasonic cleaner for 30 min. The solution was then diluted with ethanol to a slightly yellow color. A small amount of the solution was dripped onto a silicon wafer and allowed to dry at room temperature. The thickness of a single ZIS-8TU nanosheet on the silicon wafer was measured using an atomic force microscope.

[0052] (5) The light absorption performance of the ZIS-8TU photoanode was characterized by using a UV-visible spectrophotometer. The ZIS-8TU photoanode grown on the FTO glass was directly embedded in a BaSO4 background white board to form a sample with a flat surface uniformly embedded in the BaSO4 background white board for testing. The test range was 200-800nm ​​and the spectral bandwidth was 5nm.

[0053] (6) The optical properties of the ZIS-8TU photoanode were characterized by photoluminescence spectroscopy. The ZIS-8TU photoanode grown on FTO glass was directly used for testing with an excitation wavelength of 440 nm and a test range of 460 nm-640 nm.

[0054] (7) The photoelectrochemical and photodetection performance of the ZIS-8TU photoanode was tested using a three-electrode system, with the ZIS-8TU photoanode as the working electrode, the Pt electrode as the counter electrode, the Ag / AgCl electrode as the reference electrode, and the electrolyte being a mixed aqueous solution of 0.5 M Na2SO4 and 0.2 M Na2SO3 (pH = 9.6). An AM1.5G xenon lamp was used to simulate sunlight with an intensity of about 100 mW / cm 2 The potential test range of the linear voltammetric characteristic curve (LSV) is -0.8~0.6V (vs.Ag / AgCl) and the voltage scanning rate is 3mV / s. The photoelectric performance at different wavelengths uses a 254nm deep ultraviolet LED lamp and 355nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm and 765nm filters. The power is divided into five energy levels: Ⅰ, Ⅱ, Ⅲ, Ⅳ, and Ⅴ. The cycle of the transient light response test is 10s (5s irradiation, 5s dark).

[0055] Example 3 Preparation method of two-dimensional rhombohedral phase ZnIn2S4 nanosheet array photoanode

[0056] (1) The conductive glass FTO was ultrasonically cleaned with acetone, anhydrous ethanol, deionized water, and anhydrous ethanol for 15 minutes in sequence. After cleaning, the FTO was placed in the air to dry naturally.

[0057] (2) Weigh 34.8 mg ZnCl2, 148 mg InCl3·4H2O, and 230.7 mg CH4N2S powder into a beaker, add 18 mL (18 g) of deionized water, and stir with a magnetic stirrer to obtain a completely dissolved uniform precursor solution.

[0058] (3) Stick a high temperature resistant tape on one end of the conductive surface of the conductive glass FTO in step (1) to keep the conductive surface 1 cm 2 , then placed in a plasma cleaning machine with the conductive surface facing up, with a plasma treatment power of 60W for 120s. Within 10min of the effective time, two FTO sheets were placed in a polytetrafluoroethylene liner in a V-shaped conductive surface facing down, and the precursor solution prepared in step (2) was added. Placed in a forced air drying oven and heated at 170°C for 12h. After the reaction was completed, the sample was taken out and the surface impurities were repeatedly washed with deionized water and anhydrous ethanol. The obtained ZnIn2S4 photoanode sample was marked as ZIS-12TU.

[0059] (4) The ZIS-12TU nanosheets grown on the FTO surface were peeled off into ethanol and ultrasonicated in an ultrasonic cleaner for 30 min. The solution was then diluted with ethanol to a slightly yellow color. A small amount of the solution was dripped onto a silicon wafer and allowed to dry at room temperature. The layer thickness of a single ZIS-12TU nanosheet on the silicon wafer was measured using an atomic force microscope.

[0060] (5) The light absorption performance of the ZIS-12TU photoanode was characterized by using a UV-visible spectrophotometer. The ZIS-12TU photoanode grown on the FTO glass was directly embedded in a BaSO4 background white board to form a sample with a flat surface that was uniformly embedded in the BaSO4 background white board for testing. The test range was 200-800nm ​​and the spectral bandwidth was 5nm.

[0061] (6) The optical properties of the ZIS-12TU photoanode were characterized by photoluminescence spectroscopy. The ZIS-12TU photoanode grown on FTO glass was directly tested with an excitation wavelength of 440 nm and a test range of 460 nm-640 nm.

[0062] (7) The photoelectrochemical and photodetection performances of the ZIS-12TU photoanode were tested using a three-electrode system, with the ZIS-12TU photoanode as the working electrode, the Pt electrode as the counter electrode, the Ag / AgCl electrode as the reference electrode, and the electrolyte being a mixed aqueous solution of 0.5 M Na2SO4 and 0.2 M Na2SO3 (pH = 9.6). An AM1.5G xenon lamp was used to simulate sunlight with an intensity of about 100 mW / cm 2The potential test range of the linear voltammetric characteristic curve (LSV) is -0.8~0.6V (vs.Ag / AgCl), and the voltage scanning rate is 3mV / s. The photoelectric performance at different wavelengths uses a 254nm deep ultraviolet LED lamp and 355nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm and 765nm filters. The power size is divided into five energy levels: Ⅰ, Ⅱ, Ⅲ, Ⅳ, and Ⅴ. The cycle of the transient light response test is 10s (5s irradiation, 5s dark).

[0063] Example 4 Preparation method of two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode

[0064] (1) The conductive glass FTO was ultrasonically cleaned with acetone, anhydrous ethanol, deionized water, and anhydrous ethanol for 15 minutes in sequence. After cleaning, the FTO was placed in the air to dry naturally.

[0065] (2) Weigh 34.8 mg ZnCl2, 148 mg InCl3·4H2O and 307.6 mg CH4N2S powder into a beaker, add 18 mL (18 g) of deionized water, and stir with a magnetic stirrer to obtain a completely dissolved uniform precursor solution.

[0066] (3) Stick a high temperature resistant tape on one end of the conductive surface of the conductive glass FTO in step (1) to keep the conductive surface 1 cm 2 , then placed in a plasma cleaning machine with the conductive surface facing up, with a plasma treatment power of 60W for 120s. Within 10min of the effective time, two FTO sheets were placed in a polytetrafluoroethylene liner with the conductive surface facing down in a V shape, and the precursor solution prepared in step (2) was added. Placed in a blast drying oven and heated at 170°C for 12h. After the reaction was completed, the sample was taken out and the surface impurities were repeatedly washed with deionized water and anhydrous ethanol. The obtained ZnIn2S4 photoanode sample was marked as ZIS-16TU.

[0067] (4) The ZIS-16TU nanosheets grown on the FTO surface were peeled off into ethanol and ultrasonicated in an ultrasonic cleaner for 30 min. The solution was then diluted with ethanol to a slightly yellow color. A small amount of the solution was dripped onto a silicon wafer and allowed to dry at room temperature. The thickness of a single ZIS-16TU nanosheet on the silicon wafer was measured using an atomic force microscope.

[0068] (5) The light absorption performance of the ZIS-16TU photoanode was characterized by using a UV-visible spectrophotometer. The ZIS-16TU photoanode grown on the FTO glass was directly embedded in a BaSO4 background white board to form a sample with a flat surface that was uniformly embedded in the BaSO4 background white board for testing. The test range was 200-800nm ​​and the spectral bandwidth was 5nm.

[0069] (6) The optical properties of the ZIS-16TU photoanode were characterized by photoluminescence spectroscopy. The ZIS-16TU photoanode grown on FTO glass was directly tested with an excitation wavelength of 440 nm and a test range of 460 nm-640 nm.

[0070] (7) The photoelectrochemical and photodetection performance of the ZIS-16TU photoanode was tested using a three-electrode system, with the ZIS-16TU photoanode as the working electrode, the Pt electrode as the counter electrode, the Ag / AgCl electrode as the reference electrode, and the electrolyte being a mixed aqueous solution of 0.5 M Na2SO4 and 0.2 M Na2SO3 (pH = 9.6). An AM 1.5G xenon lamp was used to simulate sunlight with an intensity of about 100 mW / cm 2 The potential test range of the linear voltammetric characteristic curve (LSV) is -0.8~0.6V (vs.Ag / AgCl), and the voltage scanning rate is 3mV / s. The photoelectric performance at different wavelengths uses a 254nm deep ultraviolet LED lamp and 355nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm and 765nm filters. The power size is divided into five energy levels: Ⅰ, Ⅱ, Ⅲ, Ⅳ, and Ⅴ. The cycle of the transient light response test is 10s (5s irradiation, 5s dark).

[0071] The following table shows the optical power values ​​of five energy levels I, II, III, IV, and V corresponding to wavelengths of 254nm, 355nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, and 765nm in the present invention.

[0072]

[0073] In the present invention, we have developed a simple method to adjust the number of atomic layers of rhombohedral phase ZnIn2S4. Threshold-limited growth is achieved by adjusting the concentration of thiourea in the precursor solution, so that the formed rhombohedral phase ZnIn2S4 nanosheets can achieve controllable regulation of the number of atomic layers. Thiourea can be used as an effective stabilizer to stabilize the formation of nanosheets. However, when thiourea is present in excess, the excess thiourea will adsorb on the surface of the native nanocrystals, thereby partially hindering the growth of oriented crystals. This leads to the inhibition of growth along the c-axis direction, which in turn leads to the limitation of the stacking of atomic layers. This forms rhombohedral phase ZnIn2S4 nanosheets with fewer layers.

[0074] Example 5 Application of two-dimensional rhombohedral phase ZnIn2S4 nanosheet array photoanode

[0075] The following steps are involved:

[0076] Constructing a PEC type self-powered photodetector, using the two-dimensional rhombus phase ZnIn2S4 nanosheet array photoanode as a working electrode of the PEC type self-powered photodetector;

[0077] The PEC type self-powered photoelectric detector also includes an electrochemical workstation, an electrolyte tank, a reference electrode and a counter electrode; an electrolyte is provided in the electrolyte tank, and the reference electrode, the working electrode and the counter electrode are suspended in the electrolyte tank, all in contact with the electrolyte and not in contact with the bottom of the electrolyte tank; the fixed ends of the reference electrode, the working electrode and the counter electrode are fixed to the cover of the electrolyte tank through the card hole, and the three electrodes are freely suspended in the electrolyte tank, about 2-3 cm away from the bottom of the electrolyte tank, so that the photoelectrochemical reaction is more sufficient.

[0078] The connection of the external circuit in the PEC type self-powered photoelectric detector includes connecting the working electrode to the positive pole of the electrochemical workstation power supply with a green electrode line; connecting the counter electrode to the negative pole of the electrochemical workstation power supply with a red electrode line; and connecting the reference electrode to the reference potentiometer with a white electrode line.

[0079] The above descriptions are only some specific implementation methods of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any person familiar with the art within the technical scope disclosed in the present invention should be covered within the protection scope of the present invention.

Claims

1. A two-dimensional rhombohedral phase ZnIn 2 S 4 Preparation method of nanosheet array photoanode, It is characterized in that The following steps are involved: (1) Obtain clean conductive glass FTO; (2) Mix the following raw materials according to the preset ratio: ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 S, dissolved in water to obtain a precursor solution; (3) subjecting the conductive glass FTO conductive surface described in step (1) to plasma surface treatment; Within the effective time after the plasma surface treatment, two FTO sheets are placed in a reaction container with the conductive surface facing downward in a "V" shape, and the precursor solution prepared in step (2) is added to perform a hydrothermal reaction to obtain a two-dimensional rhombohedral ZnIn phase on the conductive surface of the conductive glass FTO. 2 S 4 Nanosheet arrays; Conductive glass FTO together with the conductive surface of conductive glass FTO to obtain a two-dimensional rhombohedral phase ZnIn 2 S 4 Nanosheet arrays, together as photoanodes, are used to make working electrodes for PEC-type self-powered photodetectors; the prepared two-dimensional rhombohedral ZnIn 2 S 4 The nanosheet array photoanode comprises: conductive glass FTO and a two-dimensional rhombus phase ZnIn in-situ grown on the conductive surface of the conductive glass FTO 2 S 4 Nanosheet array; the two-dimensional rhombohedral phase ZnIn 2 S 4 Nanosheet arrays are composed of two-dimensional rhombohedral ZnIn 2 S 4 Nanosheet stacking composition; the two-dimensional rhombus phase ZnIn 2 S 4 The layer thickness of the nanosheets is 4 nm to 44.8 nm.

2. A two-dimensional rhombohedral phase ZnIn as claimed in claim 1 2 S 4 Preparation method of nanosheet array photoanode, It is characterized in that In step (2), the setting of the preset ratio includes the following steps: Obtaining the wavelength range of the detection target of the PEC type self-powered photoelectric detector; setting the preset ratio according to the wavelength range of the detection target; When the wavelength range of the detection target is 355-765nm, the ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 The preset molar ratio of S is: 1:2:4; When the wavelength range of the detection target is 254-355nm, the ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 The preset molar ratio of S is: 1:2:

16.

3. A two-dimensional rhombohedral phase ZnIn as claimed in claim 1 2 S 4 Preparation method of nanosheet array photoanode, It is characterized in that In step (3), The reaction container is a polytetrafluoroethylene liner; the hydrothermal reaction specifically comprises: placing the polytetrafluoroethylene liner in a high-pressure reactor and performing a hydrothermal reaction at a temperature of 170° C. for 12 hours; The plasma treatment specifically includes the following steps: treating in a plasma cleaning machine with a power of 60 W and a time of 120 s; The effective time refers to the time after the plasma treatment when the conductive glass FTO surface has energy, which can promote the growth of the compound on the FTO surface. The effective time is 10 minutes.

4. A two-dimensional rhombohedral ZnIn prepared by the method according to any one of claims 1 to 3 2 S 4 Photoelectric detection applications of nanosheet array photoanodes, It is characterized in that The following steps are involved: Constructing a PEC-type self-powered photodetector using the two-dimensional rhombohedral phase ZnIn 2 S 4 Nanosheet array photoanode as the working electrode of PEC-type self-powered photodetector; The PEC type self-powered photoelectric detector also includes an electrochemical workstation, an electrolyte tank, a reference electrode and a counter electrode; an electrolyte is provided in the electrolyte tank, and the reference electrode, the working electrode and the counter electrode are suspended in the electrolyte tank, all in contact with the electrolyte, and none of them touch the bottom of the electrolyte tank; The working electrode is connected to the positive pole of the power supply of the electrochemical workstation, the counter electrode is connected to the negative pole of the power supply of the electrochemical workstation, and the reference electrode is connected to the reference potentiometer of the electrochemical workstation.

5. The photoelectric detection application as claimed in claim 4, It is characterized in that The electrolyte in the electrolyte is 0.5M Na 2 SO 4 and 0.2M Na 2 SO 3 ; The reference electrode is an Ag / AgCl electrode; and the counter electrode is a Pt electrode.

6. A two-dimensional rhombohedral phase ZnIn 2 S 4 A method for controlling the thickness of nanosheets of a nanosheet array photoanode, wherein the two-dimensional rhombus phase ZnIn 2 S 4 The nanosheet array photoanode is prepared using the preparation method as described in any one of claims 1 to 3, It is characterized in that The two-dimensional rhombohedral ZnIn phase obtained on the conductive surface of the conductive glass FTO in step (3) is adjusted by adjusting the preset ratio in step (2). 2 S 4 The layer thickness of the nanosheets; When the ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 When the preset molar ratio of S is 1:2:4, the two-dimensional rhombohedral phase ZnIn 2 S 4 The layer thickness of the nanosheet is 44.8 nm; When the ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 When the preset molar ratio of S is 1:2:8, the two-dimensional rhombohedral phase ZnIn 2 S 4 The layer thickness of the nanosheet is 18.6 nm; When the ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 When the preset molar ratio of S is 1:2:12, the two-dimensional rhombohedral phase ZnIn 2 S 4 The layer thickness of the nanosheet is 11.5 nm; When the ZnCl 2 、InCl 3 ·4H 2 O and CH 4 N 2 When the preset molar ratio of S is 1:2:16, the two-dimensional rhombohedral phase ZnIn 2 S 4 The layer thickness of the nanosheets is 4 nm.

Citation Information

Patent Citations

  • Peony-flower-shaped heterostructure micro-sphere photocatalyst and preparation and application thereof

    CN105214690A

  • ZnIn2S4 Nanosheet array structure and preparation method thereof

    CN108409157A

  • Zinc indium sulfur / copper indium sulfur two-dimensional heterojunction photocatalyst and preparation method and application thereof

    CN109589991A

  • Hydroquinone molecular imprinting photoelectrochemical sensor as well as preparation method and application thereof

    CN115343339A

  • Preparation method of two-dimensional hexagonal-phase and rhombic-phase ZnIn2S4 complex heterojunction photoelectrode

    CN115424866A