Ultraviolet detector based on amorphous copper oxide / gallium oxide heterogeneous pn junction and preparation method thereof

By growing an amorphous CuO layer on the Ga2O3 film, forming CuO/Ga2O3 heterogeneous pn junction, and separating photogenerated electron hole pairs using a built-in electric field, the dark current and response time problems of the Ga2O3 ultraviolet detector are solved, and self-powered and Efficient response improves device performance.

CN119008761APending Publication Date: 2024-11-22ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411099198.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing daily blind ultraviolet detectors prepared based on Ga2O3 materials have performance problems such as large dark current and long light response time, and require an applied voltage to detect, which limits its application.

Method used

Amorphous copper oxide/gallium oxide heterogeneous pn junction structure is adopted. By growing amorphous CuO film at low temperature on the Ga2O3 film, O2 is used as the oxygen source to compensate for the oxygen vacancy, CuO/Ga2O3 heterogeneous pn junction is formed, and a built-in electric field is used. Separate photogenerated electron hole pairs to achieve self-power supply and rapid response.

Benefits of technology

It realizes performance of light-darkness ratio, low dark current, and fast light response speed, simplifies the preparation process, reduces costs, and effectively responds to deep ultraviolet light without external power supply.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008761A_ABST
    Figure CN119008761A_ABST
Patent Text Reader

Abstract

The invention discloses an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterogeneous pn junction and a preparation method of the ultraviolet detector. The ultraviolet detector structurally comprises a c-plane sapphire substrate (c-Al2O3), a Ga2O3 thin film, an amorphous CuO thin film and a Ti / Au electrode pair in sequence from bottom to top. A pulse laser deposition method is adopted for preparation, a Ga2O3 thin film is prepared on a c-Al2O3 substrate through a PLD method, then a layer of amorphous CuO thin film is deposited at a low temperature, a CuO / Ga2O3 heterogeneous pn junction is formed, and finally a Ti / Au electrode is plated on the surface of the thin film to complete manufacturing of the heterogeneous pn junction ultraviolet detector. According to the ultraviolet detector, the CuO / Ga2O3 heterojunction is constructed, and the potential barrier and the built-in electric field at the heterojunction interface are utilized, so that the dark current of the device is greatly reduced while the self-powered function is realized; and the preparation method is simple, high in repeatability, low in cost and high in response speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterogeneous pn junction and a preparation method thereof, belonging to the technical field of semiconductor photoelectric devices. Background Art

[0002] Gallium oxide (Ga2O3) is a wide bandgap semiconductor with a direct bandgap width of about 4.9eV. The corresponding light absorption wavelength is about 250nm, which belongs to the solar-blind light band (200-280nm) and is not affected by the background noise of sunlight. At the same time, Ga2O3 material has excellent chemical and thermal stability and high transmittance in the ultraviolet and visible light ranges. It is a natural ideal material for preparing solar-blind ultraviolet detectors. Photodetectors prepared using Ga2O3 have important application prospects in military and civilian fields such as solar-blind ultraviolet communications, missile tracking, deep space detection imaging, ozone hole detection and fire risk warning. In addition, Ga2O3-based devices have excellent characteristics such as high breakdown field strength, low energy consumption, low noise, and high temperature resistance. They are also widely used in the fields of high temperature, high frequency, radiation resistance, and high-power devices.

[0003] However, in the application of solar-blind ultraviolet detectors, the comprehensive performance of MSM ultraviolet detectors based on Ga2O3 materials is still relatively low, and there are technical problems such as large dark current and long light response time. In addition, external voltage is usually required to detect the performance, so commercial applications have not been achieved. The preparation of Ga2O3-based homogeneous pn junction ultraviolet detectors seems to be a feasible alternative. However, due to the presence of defects such as oxygen vacancies, intrinsic β-Ga2O3 usually exhibits n-type conductivity, and due to low hole mobility, self-compensation effect and large formation energy of p-type dopants, Ga2O3 materials are difficult to achieve efficient p-type doping, which limits the development of its homogeneous pn junction in the field of semiconductor optoelectronic devices. It is necessary to find other p-type materials to form heterogeneous pn junctions with it. The inevitable lattice mismatch phenomenon at the interface of the crystal heterojunction will lead to carrier capture problems at the interface, resulting in high dark current and slow response speed of the device. These reasons limit the application of Ga2O3 materials in solar-blind ultraviolet detectors. Summary of the invention

[0004] In order to solve the problems of large dark current and long light response time of ultraviolet detectors, the present invention provides an ultraviolet detector based on amorphous copper oxide / gallium oxide heterogeneous pn junction and a preparation method thereof. The Ga2O3-based heterogeneous pn junction ultraviolet detector has the performance of large light-to-dark ratio, low dark current and fast light response speed, and is prepared by physical vapor deposition, and the preparation method is simple, highly repeatable and low cost.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions.

[0006] The present invention introduces O2 as an oxygen source during the film growth process to compensate for oxygen vacancies in the Ga2O3 film and the CuO film, and uses a pulsed laser deposition (PLD) method to grow an amorphous CuO film on the Ga2O3 film at a relatively low temperature to prepare an amorphous copper oxide (CuO) / gallium oxide (Ga2O3) heterogeneous pn junction, which is applied in a solar-blind ultraviolet detector. The preparation method is simple, highly repeatable, and low in cost, and the prepared detector has the characteristics of self-power supply, large light-to-dark ratio, low dark current, and fast light response speed.

[0007] Specifically, the present invention provides an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterogeneous pn junction, wherein the ultraviolet detector based on an amorphous copper oxide / gallium oxide heterogeneous pn junction comprises a c-Al2O3 substrate, a Ga2O3 film, a CuO film and a Ti / Au electrode pair, wherein c-Al2O3 is a substrate, the Ga2O3 film is arranged on the substrate c-Al2O3, the CuO film is arranged on the Ga2O3 film and covers a partial area of ​​the Ga2O3 film to form a heterogeneous pn junction region, and the Ti / Au electrode pair comprises two Ti / Au electrodes, one is arranged on the pn junction region, i.e., the CuO film, and the other is arranged on a single-layer Ga2O3 film.

[0008] Further preferably, the amorphous copper oxide / gallium oxide heterojunction pn junction ultraviolet detector is characterized by comprising:

[0009] c-Al2O3 substrate;

[0010] The Ga2O3 film layer disposed on the c-Al2O3 substrate:

[0011] An amorphous CuO film layer and a first Ti / Au electrode are disposed on the Ga2O3 film layer;

[0012] A second Ti / Au electrode is disposed on the amorphous CuO film layer.

[0013] The Ga2O3 film layer is an n-type semiconductor, and the amorphous CuO film layer is a p-type semiconductor.

[0014] The thickness of the Ga2O3 film layer is 100-200nm, and the thickness of the amorphous CuO film layer is 20-70nm.

[0015] The first Ti / Au electrode includes a Ti layer grown on the Ga2O3 film layer and an Au layer grown on the Ti layer;

[0016] The second Ti / Au electrode includes a Ti layer grown on the amorphous CuO film layer and an Au layer grown on the Ti layer.

[0017] Copper oxide (CuO) is a traditional p-type material with a bandgap of about 1.9 eV, high hole mobility, and can achieve rapid current transmission. The present invention introduces CuO and Ga2O3 to construct a heterogeneous pn junction, and utilizes the built-in electric field formed at the interface of the two materials to accelerate the separation of photogenerated electron-hole pairs. In the absence of an external power source, the device can respond to deep ultraviolet light. In addition, the device performance of the ultraviolet detector, such as responsiveness, response speed, and sensitivity, can be effectively improved. During the growth of the Ga2O3 film and the CuO film, the present invention introduces high-purity O2 as an oxygen source, which effectively reduces the oxygen vacancy concentration in the film, reduces the carrier concentration of the intrinsic film, and greatly reduces the dark current of the device. At the same time, the present invention prepares an amorphous CuO film at a relatively low temperature, effectively reduces the lattice mismatch problem at the heterojunction interface, and reduces the probability of carrier capture at the interface.

[0018] The present invention also provides a method for preparing the above-mentioned amorphous copper oxide / gallium oxide heterogeneous pn junction ultraviolet detector, comprising the following steps:

[0019] 1) Depositing a Ga2O3 film on the surface of the c-Al2O3 substrate by laser pulse deposition;

[0020] 2) Amorphous CuO film is deposited on a part of the Ga2O3 film by laser pulse deposition. The Ga2O3 film and the amorphous CuO film form a CuO / Ga2O3 heterogeneous pn junction region.

[0021] 3) A first Ti / Au electrode is evaporated on a portion of the remaining area of ​​the Ga2O3 film layer, and a second Ti / Au electrode is evaporated on the amorphous CuO film layer in the CuO / Ga2O3 heterogeneous pn junction area. The first Ti / Au electrode and the second Ti / Au electrode form a Ti / Au electrode pair to complete the preparation.

[0022] In step 1), a Ga2O3 film layer is deposited on the surface of the c-Al2O3 substrate by laser pulse deposition, which specifically includes:

[0023] Fix the Ga2O3 target on the target stage in the laser pulse deposition chamber, fix the cleaned c-Al2O3 substrate on the sample stage, adjust the distance between the target and the substrate to 4-8 cm, and separate the target and the substrate with a baffle;

[0024] Close the vent valve and chamber door in sequence, and turn on the mechanical pump and molecular pump in sequence to make the chamber reach 1.0×10 -3 Pa vacuum degree; then set the temperature rising program, heat the c-Al2O3 substrate to 600-700℃, and maintain the temperature stable; introduce O2 into the vacuum chamber, adjust the pressure, and keep the pressure in the chamber at 0.07-0.2Pa;

[0025] Turn on the laser, preheat for 5-15 minutes and adjust the laser to constant energy mode, then adjust the laser energy to 180-220 mJ / cm 2 , the laser frequency is 1-5Hz; adjust the target position so that the laser beam is focused on the Ga2O3 target surface and ablate the target to form a plume; turn on the rotation of the target and the sample stage, first perform pre-deposition for 3-20min to remove the non-stoichiometric part of the target surface, then open the baffle between the target and the substrate, deposit the Ga2O3 film on the surface of the c-Al2O3 substrate for 30-90min, and anneal after deposition to obtain the Ga2O3 film. The annealing conditions are: rapid annealing at 750℃~850℃ for 20-40min in N2 atmosphere.

[0026] In step 2), an amorphous CuO film layer is deposited on a partial area of ​​the Ga2O3 film layer by using a laser pulse deposition method, specifically comprising:

[0027] The CuO target is fixed on the target stage in the PLD chamber, a mask is attached to a part of the Ga2O3 film prepared in step 1), fixed on the sample stage, the distance from the target to the substrate is adjusted to 4-8 cm, and the target and the Ga2O3 film are separated by a baffle;

[0028] Close the vent valve and chamber door in sequence, and turn on the mechanical pump and molecular pump in sequence to make the chamber reach 1.0×10 -3 Pa vacuum degree; then set the temperature rising program, heat the Ga2O3 film to 100℃-400℃, and maintain the temperature stable; introduce O2 into the vacuum chamber, adjust the pressure, and keep the pressure in the chamber at 0.3~0.7Pa;

[0029] Turn on the laser and adjust the laser energy to 180-220 mJ / cm 2 , the laser frequency is 1 to 3 Hz; adjust the target position so that the laser beam is focused on the CuO target surface and ablate the target to form a plume; turn on the rotation of the target and the sample stage, first perform pre-deposition for 3-20 minutes to remove the non-stoichiometric portion of the target surface, then open the baffle between the target and the substrate, and deposit a CuO film on the area of ​​the Ga2O3 film where the mask plate is not attached. The deposition time is 30-90 minutes to form a CuO / Ga2O3 heterogeneous pn junction region.

[0030] In step 3), a first Ti / Au electrode is deposited on a portion of the remaining area of ​​the Ga2O3 film layer, and a second Ti / Au electrode is deposited on the amorphous CuO film layer in the CuO / Ga2O3 heterogeneous pn junction region, specifically comprising:

[0031] The CuO / Ga2O3 heterogeneous pn junction area and the single-layer Ga2O3 film prepared in step 2) are attached with a mask and fixed on the sample stage. Electron beam evaporation technology is first used to A Ti layer with a thickness of 15 to 25 nm is grown at a speed of 1000 nm, and then electron beam evaporation technology is used to An Au layer with a thickness of 40 to 60 nm is grown at a rate of

[0032] Further preferably, the specific preparation steps are as follows: 1) using the PLD method to deposit Ga2O3 thin film on the surface of the c-Al2O3 substrate: fix the Ga2O3 target on the target stage in the chamber, fix the cleaned c-Al2O3 substrate on the sample stage, adjust the distance from the target to the substrate to 6.0 cm, and separate the target and the substrate with a baffle; close the vent valve and the chamber door in turn, turn on the mechanical pump and the molecular pump in turn, and reach the required 10 after about 2 hours. -4 Pa vacuum degree; then heat the c-Al2O3 substrate to 650℃ and maintain the temperature stable; introduce O2 into the vacuum chamber and adjust the pressure to keep it at 0.1Pa; turn on the laser, preheat for 10min and adjust the laser to constant energy mode, and then adjust the laser energy to 200mJ / cm 2 , the laser frequency is 3Hz; the target position is adjusted to focus the laser beam on the Ga2O3 target surface and ablate the target to form a plume; the rotation of the target and the sample stage is turned on, and a pre-deposition is performed for 5-10 minutes to remove the non-stoichiometric portion of the target surface, and then the baffle between the target and the substrate is opened to deposit a Ga2O3 film on the surface of the c-Al2O3 substrate to obtain a Ga2O3 film; the obtained Ga2O3 film is rapidly annealed at 800°C in a N2 atmosphere for 30 minutes to eliminate some stress in the film and improve the quality of the Ga2O3 film.

[0033] 2) CuO thin film is deposited on a part of the Ga2O3 thin film by PLD method to form a heterogeneous pn junction region: the CuO target is fixed on the target stage in the chamber, a mask is attached to the Ga2O3 thin film prepared in step 1), and it is fixed on the sample stage, the distance from the target to the Ga2O3 thin film is adjusted to 6.0 cm, and the target and the Ga2O3 thin film are separated by a baffle; the vent valve and the chamber door are closed in turn, and the mechanical pump and the molecular pump are opened in turn. After about 2 hours, the required 10 -4 Pa vacuum degree; then heat the Ga2O3 film to 100℃-400℃ and maintain the temperature stable; introduce O2 into the vacuum chamber and adjust the pressure to keep it at 0.5Pa; turn on the laser and adjust the laser energy to 200mJ / cm 2, the laser frequency is 1Hz; adjust the target position so that the laser beam is focused on the CuO target surface and ablate the target to form a plume; turn on the rotation of the target and the sample stage, perform pre-deposition for 5-10 minutes to remove the non-stoichiometric portion of the target surface, then open the baffle between the target and the Ga2O3 film, and deposit the CuO film on the area of ​​the Ga2O3 film where the mask is not attached to obtain a CuO / Ga2O3 heterogeneous pn junction.

[0034] In steps 1) and 2), the PLD deposition time of the Ga2O3 film and the CuO film can be adjusted in the range of 30-90 minutes, and a Ga2O3 film with a thickness of 100-200 nm and a CuO film with a thickness of 20-70 nm can be obtained respectively.

[0035] 3) A mask is attached to the CuO / Ga2O3 heterogeneous pn junction region and a part of the single Ga2O3 film prepared in step 2), and the mask is fixed on the sample stage. Electron beam evaporation is used to deposit the CuO / Ga2O3 heterogeneous pn junction region and the single Ga2O3 film surface with and Ti / Au electrodes with thicknesses of 20 nm and 50 nm were grown at a rate of , forming a Ti / Au electrode pair, completing the preparation of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector.

[0036] The working principle of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector of the present invention is: utilizing the characteristics of the built-in electric field at the interface of the CuO / Ga2O3 heterogeneous pn junction to effectively separate photogenerated electron-hole pairs. Under the condition of no external power supply, the current in a dark environment is at the pA level; after irradiating the device with 254nm day-blind light, the Ga2O3 film generates a large number of photogenerated electron-hole pairs, which are accelerated and separated under the action of the built-in electric field, resulting in an increase in photocurrent, thereby realizing the self-powered characteristic of the device.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] 1) The Ga2O3 film and the CuO film of the present invention are both prepared by PLD technology, which has a simple preparation process, high repeatability, and a safe and non-toxic preparation process. The CuO / Ga2O3 heterojunction has an obvious response to 254nm wavelength light, which belongs to the solar-blind ultraviolet range, is not affected by sunlight, and can be used all day long.

[0039] 2) The present invention successfully applies the CuO / Ga2O3 heterogeneous pn junction prepared by PLD technology in ultraviolet detectors, and has excellent performances such as photoresponsivity, photoresponse time, and sensitivity.

[0040] 3) The present invention uses O2 as an oxygen source during film growth, effectively reducing the oxygen vacancy concentration in Ga2O3 film and CuO film; at the same time, since the CuO film is obtained at a lower temperature, the oxygen vacancy concentration therein can be further suppressed. Fewer oxygen vacancies can reduce the carrier concentration of the intrinsic film and the dark current of the device, while also inhibiting the capture of photogenerated carriers and promoting their separation, thereby improving the response speed of the device.

[0041] 4) The amorphous CuO film prepared at a lower temperature has a smooth and dense surface. At the same time, the amorphous structure can effectively avoid the carrier capture effect caused by lattice mismatch at the interface of the heterojunction.

[0042] 5) Compared with the traditional single-layer Ga2O3-based ultraviolet detector, the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector of the present invention realizes the effective separation of photogenerated electron-hole pairs without an external power supply through the built-in electric field formed between the two materials, effectively improves the light response speed of the device, and realizes the self-powered characteristic of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a front view structural schematic diagram of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector of the present invention.

[0044] Figure 2 It is a schematic diagram of the top view structure of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector of the present invention.

[0045] Figure 3 This is the XRD diagram of the amorphous CuO film of the present invention.

[0046] Figure 4 This is the IV curve of the CuO / Ga2O3 heterogeneous pn junction UV detector prepared in Example 1, using a light wavelength of 254nm and a power of 197μW / cm 2 of ultraviolet light.

[0047] Figure 5 This is an enlarged view of the light response time curve of the CuO / Ga2O3 heterogeneous pn junction UV detector prepared in Example 1. Under 0V bias, the light wavelength is 254nm and the power is 197μW / cm 2 of ultraviolet light.

[0048] Figure 6 This is the IV curve of the CuO / Ga2O3 heterogeneous pn junction UV detector prepared in Example 2, using a light wavelength of 254nm and a power of 197μW / cm 2 of ultraviolet light.

[0049] Figure 7This is an enlarged view of the light response time curve of the CuO / Ga2O3 heterogeneous pn junction UV detector prepared in Example 2. Under 0V bias, the light wavelength is 254nm and the power is 197μW / cm 2 of ultraviolet light. DETAILED DESCRIPTION

[0050] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0051] like Figure 1 , Figure 2 , respectively, are the front view and top view of the structure of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector of the present invention. Figure 1 and 2 The structure of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector of the present invention is a c-Al2O3 substrate, a Ga2O3 film, a CuO film and a Ti / Au electrode pair from bottom to top.

[0052] Example 1

[0053] 1) Fix the 99.99% pure Ga2O3 target on the target stage in the chamber, fix the cleaned c-Al2O3 substrate on the sample stage, adjust the distance between the target and the substrate to 6.0 cm, and separate the target and the substrate with a baffle. Close the vent valve and the chamber door in turn, turn on the mechanical pump and the molecular pump in turn, and reach the required 10 after about 2 hours. -4 Pa vacuum degree. Set the temperature program, heat the c-Al2O3 substrate to 650℃, and maintain the temperature stable; introduce O2 into the vacuum chamber and adjust the pressure to keep the pressure in the chamber at 0.1Pa. Then turn on the laser, preheat for 10min and adjust the laser to constant energy mode, and then adjust the laser energy to 200mJ / cm 2 , adjust the laser frequency to 3Hz, adjust the target position so that the laser beam is focused on the Ga2O3 target surface and ablate the target to form a plume. Turn on the rotation of the target and the sample stage, open the baffle between the target and the substrate after pre-deposition for 5-10 minutes, and deposit the Ga2O3 film on the surface of the c-Al2O3 substrate for 60 minutes. After the deposition is completed, turn off the laser and keep it at 650℃ for 30 minutes. Turn off the heater, turn off the vacuum system after naturally cooling to room temperature, and then perform rapid thermal annealing at 800℃ for 30 minutes in a N2 atmosphere to obtain a 150nm thick Ga2O3 polycrystalline film.

[0054] 2) Fix the 99.99% CuO target on the target stage in the chamber, paste the mask on the Ga2O3 film prepared in step 1), fix it on the sample stage, adjust the distance between the target and the substrate to 6.0 cm, and separate the target and the Ga2O3 film with a baffle. Close the vent valve and the chamber door in turn, turn on the mechanical pump and the molecular pump in turn, and reach the required 10 after about 2 hours. -4 Pa vacuum degree. Heat the Ga2O3 film to 250℃ and maintain the temperature stable; introduce O2 into the vacuum chamber and adjust the pressure to keep the pressure in the chamber at 0.5Pa. Turn on the laser, preheat for 10min and adjust the laser to constant energy mode, then adjust the laser energy to 200mJ / cm 2 , adjust the laser frequency to 1Hz, adjust the target position so that the laser beam is focused on the CuO target surface and ablate the target to form a plume. Turn on the rotation of the target and the sample stage, open the baffle between the target and the Ga2O3 film after pre-deposition for 5-10 minutes, and deposit the CuO film on part of the Ga2O3 film for 60 minutes. After the deposition is completed, turn off the laser and keep it at 250°C for 30 minutes. Turn off the heater, cool it down naturally to room temperature, and then turn off the vacuum system to obtain a 50nm thick amorphous CuO film. The crystallinity of the film is as follows Figure 3 shown.

[0055] 3) A mask was attached to the CuO / Ga2O3 heterogeneous pn junction region and a part of the upper region of the single-layer Ga2O3 film prepared in step 2), and the mask was fixed on the sample stage. and Ti / Au electrodes with thicknesses of 20 nm and 50 nm were grown at a rate to form a Ti / Au electrode pair and obtain a CuO / Ga2O3 heterogeneous pn junction ultraviolet detector.

[0056] like Figure 4 The IV curve of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector prepared in this embodiment is shown in FIG. Figure 5 The photoresponse time curve of the CuO / Ga2O3 heterogeneous pn junction UV detector prepared in this embodiment under 0V bias is enlarged, and the light wavelength is 254nm and the power is 197μW / cm 2 As shown in the figure, the CuO / Ga2O3 heterojunction UV detector prepared in this example has a dark current of 2.05pA and a responsivity of 3.62mA / W under a bias voltage of 0V, and the corresponding response time constant is τ r =539ms; τ d =115ms.

[0057] Example 2

[0058] 1) Fix the 99.99% pure Ga2O3 target on the target stage in the chamber, fix the cleaned c-Al2O3 substrate on the sample stage, adjust the distance between the target and the substrate to 6.0 cm, and separate the target and the substrate with a baffle. Close the vent valve and the chamber door in turn, turn on the mechanical pump and the molecular pump in turn, and reach the required 10 after about 2 hours. -4 Pa vacuum degree. Set the temperature program, heat the c-Al2O3 substrate to 650℃, and maintain the temperature stable; introduce O2 into the vacuum chamber and adjust the pressure to keep the pressure in the chamber at 0.1Pa. Then turn on the laser, preheat for 10min and adjust the laser to constant energy mode, and then adjust the laser energy to 200mJ / cm 2 , adjust the laser frequency to 3Hz, adjust the target position so that the laser beam is focused on the Ga2O3 target surface and ablate the target to form a plume. Turn on the rotation of the target and the sample stage, open the baffle between the target and the substrate after pre-deposition for 5-10 minutes, and deposit the Ga2O3 film on the surface of the c-Al2O3 substrate for 60 minutes. After the deposition is completed, turn off the laser and keep it at 650℃ for 30 minutes. Turn off the heater, turn off the vacuum system after naturally cooling to room temperature, and then perform rapid thermal annealing at 800℃ for 30 minutes in a N2 atmosphere to obtain a 150nm thick Ga2O3 polycrystalline film.

[0059] 2) Fix the 99.99% CuO target on the target stage in the chamber, paste the mask on the Ga2O3 film prepared in step 1), fix it on the sample stage, adjust the distance between the target and the substrate to 6.0 cm, and separate the target and the Ga2O3 film with a baffle. Close the vent valve and the chamber door in turn, turn on the mechanical pump and the molecular pump in turn, and reach the required 10 after about 2 hours. -4 Pa vacuum degree. Heat the Ga2O3 film to 350℃ and maintain the temperature stable; introduce O2 into the vacuum chamber and adjust the pressure to keep the pressure in the chamber at 0.5Pa. Turn on the laser, preheat for 10min and adjust the laser to constant energy mode, then adjust the laser energy to 200mJ / cm 2 , adjust the laser frequency to 1Hz, adjust the target position so that the laser beam is focused on the CuO target surface and ablate the target to form a plume. Turn on the rotation of the target and the sample stage, open the baffle between the target and the Ga2O3 film after pre-deposition for 5-10 minutes, and deposit the CuO film on part of the Ga2O3 film for 60 minutes. After the deposition is completed, turn off the laser and keep it at 350℃ for 30 minutes. Turn off the heater, cool it down naturally to room temperature, and then turn off the vacuum system to obtain a 50nm thick amorphous CuO film. The crystallinity of the film is as follows Figure 3 shown.

[0060] 3) A mask was attached to the CuO / Ga2O3 heterogeneous pn junction region and a part of the upper region of the single-layer Ga2O3 film prepared in step 2), and the mask was fixed on the sample stage. and Ti / Au electrodes with thicknesses of 20 nm and 50 nm were grown at a rate to form a Ti / Au electrode pair and obtain a CuO / Ga2O3 heterogeneous pn junction ultraviolet detector.

[0061] like Figure 6 The IV curve of the CuO / Ga2O3 heterogeneous pn junction ultraviolet detector prepared in this embodiment is shown in FIG. Figure 7 The photoresponse time curve of the CuO / Ga2O3 heterogeneous pn junction UV detector prepared in this embodiment under 0V bias is enlarged, and the light wavelength is 254nm and the power is 197μW / cm 2 As shown in the figure, the CuO / Ga2O3 heterojunction UV detector prepared in this example has a dark current of 0.87pA and a responsivity of 8.14mA / W under a bias voltage of 0V. The corresponding response time constant is τ r =335ms; τ d =103ms.

[0062] On the basis of the above embodiments, by adjusting the PLD deposition time of Ga2O3 film and CuO film to 30-90min, a Ga2O3 film with a thickness of 100-200nm and a CuO film with a thickness of 20-70nm can be obtained respectively. Within this thickness range, the heterogeneous pn junction formed by the Ga2O3 film and the CuO film can achieve the technical effects of the above embodiments and meet the purpose of the invention.

[0063] The above description is only a partial embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the above disclosed methods and technical contents without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. An ultraviolet detector based on amorphous copper oxide / gallium oxide heterojunction pn junction, characterized in that: include: c-Al2O3 substrate; The Ga2O3 film layer disposed on the c-Al2O3 substrate: An amorphous CuO film layer and a first Ti / Au electrode are disposed on the Ga2O3 film layer; A second Ti / Au electrode is disposed on the amorphous CuO film layer.

2. The amorphous copper oxide / gallium oxide heterojunction ultraviolet detector according to claim 1, characterized in that: The Ga2O3 film layer is an n-type semiconductor, and the amorphous CuO film layer is a p-type semiconductor.

3. The ultraviolet detector based on amorphous copper oxide / gallium oxide heterojunction according to claim 1, characterized in that: The thickness of the Ga2O3 film layer is 100-200nm, and the thickness of the amorphous CuO film layer is 20-70nm.

4. The amorphous copper oxide / gallium oxide heterojunction ultraviolet detector according to claim 1, characterized in that: The first Ti / Au electrode includes a Ti layer grown on the Ga2O3 film layer and an Au layer grown on the Ti layer; The second Ti / Au electrode includes a Ti layer grown on the amorphous CuO film layer and an Au layer grown on the Ti layer.

5. The method for preparing a UV detector based on amorphous copper oxide / gallium oxide heterojunction according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) Depositing a Ga2O3 film on the surface of the c-Al2O3 substrate by laser pulse deposition; 2) Amorphous CuO film is deposited on a part of the Ga2O3 film by laser pulse deposition. The Ga2O3 film and the amorphous CuO film form a CuO / Ga2O3 heterogeneous pn junction region. 3) A first Ti / Au electrode is evaporated on a portion of the remaining area of ​​the Ga2O3 film layer, and a second Ti / Au electrode is evaporated on the amorphous CuO film layer in the CuO / Ga2O3 heterogeneous pn junction area. The first Ti / Au electrode and the second Ti / Au electrode form a Ti / Au electrode pair to complete the preparation.

6. The method for preparing an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterojunction pn junction according to claim 5, characterized in that: In step 1), a Ga2O3 film layer is deposited on the surface of the c-Al2O3 substrate by laser pulse deposition, which specifically includes: Fix the Ga2O3 target on the target stage in the laser pulse deposition chamber, fix the cleaned c-Al2O3 substrate on the sample stage, adjust the distance between the target and the substrate to 4-8 cm, and separate the target and the substrate with a baffle; Close the vent valve and chamber door in sequence, and turn on the mechanical pump and molecular pump in sequence to make the chamber reach 1.0×10 -3 Pa vacuum degree; then set the temperature rising program, heat the c-Al2O3 substrate to 600-700℃, and maintain the temperature stable; introduce O2 into the vacuum chamber, adjust the pressure, and keep the pressure in the chamber at 0.07-0.2Pa; Turn on the laser, preheat for 5-15 minutes and adjust the laser to constant energy mode, then adjust the laser energy to 180-220 mJ / cm 2 , the laser frequency is 1 to 5 Hz; the target position is adjusted so that the laser beam is focused on the Ga2O3 target surface and ablates the target to form a plume; the rotation of the target and the sample stage is turned on, and a pre-deposition is performed for 3 to 20 minutes to remove the non-stoichiometric portion of the target surface, and then the baffle between the target and the substrate is opened to deposit a Ga2O3 film on the surface of the c-Al2O3 substrate for 30 to 90 minutes, and the Ga2O3 film is annealed after deposition to obtain the Ga2O3 film.

7. The method for preparing an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterojunction according to claim 6, characterized in that: Annealing conditions are: rapid annealing at 750°C to 850°C for 20 to 40 minutes in a N2 atmosphere.

8. The method for preparing an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterojunction pn junction according to claim 5, characterized in that: In step 2), an amorphous CuO film layer is deposited on a partial area of ​​the Ga2O3 film layer by using a laser pulse deposition method, specifically comprising: The CuO target is fixed on the target stage in the PLD chamber, a mask is attached to a part of the Ga2O3 film prepared in step 1), fixed on the sample stage, the distance from the target to the substrate is adjusted to 4-8 cm, and the target and the Ga2O3 film are separated by a baffle; Close the vent valve and chamber door in sequence, and turn on the mechanical pump and molecular pump in sequence to make the chamber reach 1.0×10 -3 Pa vacuum degree; then set the temperature rising program, heat the Ga2O3 film to 100℃-400℃, and maintain the temperature stable; introduce O2 into the vacuum chamber, adjust the pressure, and keep the pressure in the chamber at 0.3~0.7Pa; Turn on the laser and adjust the laser energy to 180-220 mJ / cm 2 , the laser frequency is 1 to 3 Hz; adjust the target position so that the laser beam is focused on the CuO target surface and ablate the target to form a plume; turn on the rotation of the target and the sample stage, first perform pre-deposition for 3-20 minutes to remove the non-stoichiometric portion of the target surface, then open the baffle between the target and the substrate, and deposit a CuO film on the area of ​​the Ga2O3 film where the mask plate is not attached. The deposition time is 30-90 minutes to form a CuO / Ga2O3 heterogeneous pn junction region.

9. The method for preparing an ultraviolet detector based on an amorphous copper oxide / gallium oxide heterojunction pn junction according to claim 5, characterized in that: In step 3), a first Ti / Au electrode is deposited on a portion of the remaining area of ​​the Ga2O3 film layer, and a second Ti / Au electrode is deposited on the amorphous CuO film layer in the CuO / Ga2O3 heterogeneous pn junction region, specifically comprising: The CuO / Ga2O3 heterogeneous pn junction area and the single-layer Ga2O3 film prepared in step 2) are attached with a mask and fixed on the sample stage. Electron beam evaporation technology is first used to A Ti layer with a thickness of 15 to 25 nm is grown at a speed of 1000 nm, and then electron beam evaporation technology is used to An Au layer with a thickness of 40 to 60 nm is grown at a rate of