Processing technology of communication optical cable

By using epoxy soybean oil and other materials to prepare fiber paste and protective materials and coat them on optical cables, the problems of increasing diameter and weight of optical cables and layering are solved, and performance improvement and optimization of size and weight are achieved.

CN118981079APending Publication Date: 2024-11-19SHANDONG YIBO OPTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411249563.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing optical cable processing technology, the multi-layer fireproof layer, waterproof layer and sheath layer increase the diameter and weight of the optical cable, which can easily lead to layering and affect the use effect of the optical cable.

Method used

Fiber paste is prepared using epoxy soybean oil, gelling agent, styrene butadiene rubber and antioxidants, and protective materials are prepared through polyethylene, nanoglue powder, ultrafine magnesium oxide and reinforced fibers, and protective materials are coated through a hybrid extruder. On optical cables, enhance the performance of optical cables without increasing diameter and weight to avoid layering.

Benefits of technology

It effectively enhances the performance of optical cables, reduces diameter and weight, and avoids layering, improving the effectiveness of optical cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118981079A_ABST
    Figure CN118981079A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of communication, particularly relates to a processing technology of a communication optical cable, and aims to solve the problems that the diameter and the weight of the existing optical cable are easy to increase, the use of the optical cable is influenced and a layering phenomenon is easy to generate. The fiber paste comprises 70-90 parts by weight of epoxidized soybean oil, 2-10 parts by weight of a gelling agent, 1.0-4.0 parts by weight of styrene butadiene rubber and 0.2-1.0 part by weight of an antioxidant, the protective material comprises 75-85 parts by weight of polyethylene, 10-15 parts by weight of nano rubber powder, 1-5 parts by weight of superfine magnesium oxide and 1-5 parts by weight of reinforced fibers, the fiber paste is prepared, so that the optical cable is conveniently processed by using the fiber paste, and the optical cable is prevented from being damaged by the fiber paste. By preparing the protective material, after the protective material is coated on the optical cable, the performance of the optical cable can be enhanced, the diameter and the weight are not increased, and the layering phenomenon is not easy to generate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of communication technology, and in particular to a processing technology for communication optical cables. Background Art

[0002] The Chinese patent document with application number 201811495166.X discloses a processing and production process for optical cables, including the following steps: S1 laying-out process, S2 fiber paste coating process, S3 injection molding fireproof layer, S4 injection molding waterproof layer, S5 injection molding sheath layer. This design has the advantages of simple production process and low cost.

[0003] However, there are also some problems with the processing and production technology for optical cables. For example, the surface of the optical cable needs to be wrapped with a fireproof layer, a waterproof layer and a sheath layer. Too many wrapped layers will not only increase the diameter of the optical cable, but also increase the weight of the optical cable. Wrapping the fireproof layer, waterproof layer and sheath layer at the same time will easily lead to stratification between the fireproof layer, waterproof layer and sheath layer. Summary of the invention

[0004] Based on the problems that the background technology easily increases the diameter and weight of the optical cable, affects the use of the optical cable, and easily causes delamination, the present invention proposes a processing technology for communication optical cables.

[0005] The present invention provides a processing technology for a communication optical cable, comprising the following steps:

[0006] S1: preparing a fiber paste and a protective material, wherein the fiber paste comprises 70 to 90 parts by weight of epoxy soybean oil, 2 to 10 parts of a gelling agent, 1.0 to 4.0 parts of styrene-butadiene rubber and 0.2 to 1.0 parts of an antioxidant, and the protective material comprises 75 to 85 parts by weight of polyethylene, 10 to 15 parts of nano rubber powder, 1 to 5 parts of ultrafine magnesium oxide and 1 to 5 parts of reinforcing fiber, wherein the reinforcing fiber comprises coconut charcoal fiber and para-aramid fiber;

[0007] S2: Select an optical cable and evenly apply the fiber paste on the surface of the optical cable to obtain an optical cable coated with the fiber paste;

[0008] S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the melted liquid protective material and coat it on the surface of the optical cable. Prepare fiber paste with epoxy soybean oil, gelling agent, styrene-butadiene rubber and antioxidant, which is convenient for processing the optical cable with fiber paste. Prepare protective material with polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber. After coating the protective material on the optical cable, the performance of the optical cable can be enhanced without increasing the diameter and weight. At the same time, it is not easy to produce stratification.

[0009] Preferably, in S1, the gelling agent is a high molecular copolymer, which is a hydrogenated copolymer of ethylene compounds and rubber, so as to facilitate the molding of the material.

[0010] Preferably, in S1, styrene butadiene rubber is obtained in advance, poured into a crushing and grinding device, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain styrene butadiene rubber that passes the 200-mesh sieve, and the crushed material is convenient for material fusion.

[0011] Preferably, in S1, the preparation method of the fiber paste is as follows: obtain epoxidized soybean oil, heat the epoxidized soybean oil to 80°C, then add a gelling agent and styrene-butadiene rubber to stir and mix, use a microwave processor to reflux and stir for 9 minutes, then add an antioxidant, continue to reflux and stir for 15 minutes, stir well and evenly, continue to heat until all the materials are melted and mixed into a liquid to obtain a fiber paste, thereby facilitating the preparation of the fiber paste.

[0012] Preferably, in S1, the preparation method of ultrafine magnesium oxide is as follows: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge wash, vacuum dry at room temperature, and burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide. After the ultrafine magnesium oxide is processed, it is convenient for the materials to be fused.

[0013] Preferably, in S1, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers, which facilitates the material fusion of coconut charcoal fiber and para-aramid fiber.

[0014] Preferably, in S1, the preparation method of the protective material is as follows: polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber are poured into a mixing device and mixed evenly, and microwaved for 15 minutes to obtain the protective material, and the protective material can protect the optical cable.

[0015] Preferably, in S1, the working conditions of the microwave processor are a microwave frequency of 2450 MHz and an output power of 700 W, which facilitates the mutual mixing of the reinforcing fibers.

[0016] Preferably, in S3, the screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:1, so as to facilitate extrusion of the protective material for coating on the optical cable.

[0017] Preferably, in S3, the optical cable coated with the protective material is dried to obtain a finished communication optical cable.

[0018] Beneficial effects of the present invention:

[0019] The fiber paste is prepared by epoxy soybean oil, gelling agent, styrene-butadiene rubber and antioxidant, which makes it convenient to use the fiber paste to process the optical cable. The protective material is prepared by polyethylene, nano-rubber powder, ultrafine magnesium oxide and reinforcing fiber. After the protective material is coated on the optical cable, the performance of the optical cable can be enhanced without increasing the diameter and weight much, and it is not easy to produce stratification. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The working flow chart proposed by the present invention. DETAILED DESCRIPTION

[0021] The present invention will be further explained below in conjunction with specific embodiments.

[0022] Reference Figure 1 , Embodiment 1

[0023] This embodiment provides a processing technology for communication optical cable, including the following steps:

[0024] S1: prepare fiber paste and protective material, the weight parts of fiber paste include 86 parts of epoxy soybean oil, 10 parts of gelling agent, 3.3 parts of styrene butadiene rubber and 0.7 parts of antioxidant, the weight parts of protective material include 80 parts of polyethylene, 14 parts of nano rubber powder, 3 parts of ultrafine magnesium oxide and 3 parts of reinforcing fiber, the reinforcing fiber includes coconut charcoal fiber and para-aramid fiber, the gelling agent selects polymer copolymer, the polymer copolymer is a hydrogenated copolymer of ethylene compound and rubber, styrene butadiene rubber is obtained in advance, the styrene butadiene rubber is poured into a crushing and grinding equipment, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain styrene butadiene rubber that passes the 200-mesh sieve, the preparation method of fiber paste: obtain epoxy soybean oil, heat the epoxy soybean oil to 80°C, then add the gelling agent and styrene butadiene rubber to stir and mix, use a microwave processor to stir under microwave reflux for 9 minutes , then add an antioxidant, continue to stir under microwave reflux for 15 minutes, stir evenly, continue heating until all the materials are melted and mixed into a liquid to obtain a fiber paste, a method for preparing ultrafine magnesium oxide: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge, wash, vacuum and dry at room temperature, burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers, a method for preparing a protective material: pour polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber into a mixing device, mix evenly, and microwave for 15 minutes to obtain a protective material, and the working conditions of the microwave processor are a microwave frequency of 2450MHz and an output power of 700W;

[0025] S2: Select an optical cable and evenly coat the fiber paste on the surface of the optical cable to obtain an optical cable coated with fiber paste. The screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:1;

[0026] S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the melted protective material into liquid and coat and package it on the surface of the optical cable. The optical cable coated with the protective material can be dried to obtain a finished communication optical cable.

[0027] Reference Figure 1 , Embodiment 2

[0028] This embodiment provides a processing technology for communication optical cable, including the following steps:

[0029] S1: prepare fiber paste and protective material, the weight parts of fiber paste include 87 parts of epoxy soybean oil, 9 parts of gelling agent, 3.1 parts of styrene butadiene rubber and 0.9 parts of antioxidant, the weight parts of protective material include 79 parts of polyethylene, 12 parts of nano rubber powder, 4 parts of ultrafine magnesium oxide and 5 parts of reinforcing fiber, the reinforcing fiber includes coconut charcoal fiber and para-aramid fiber, the gelling agent selects polymer copolymer, the polymer copolymer is a hydrogenated copolymer of ethylene compound and rubber, styrene butadiene rubber is obtained in advance, the styrene butadiene rubber is poured into a crushing and grinding equipment, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain styrene butadiene rubber that passes the 200-mesh sieve, the preparation method of fiber paste: obtain epoxy soybean oil, heat the epoxy soybean oil to 80°C, then add the gelling agent and styrene butadiene rubber to stir and mix, use a microwave processor to reflux and stir for 9 minutes , then add an antioxidant, continue to stir under microwave reflux for 15 minutes, stir evenly, continue heating until all the materials are melted and mixed into a liquid to obtain a fiber paste, a method for preparing ultrafine magnesium oxide: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge, wash, vacuum and dry at room temperature, burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers, a method for preparing a protective material: pour polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber into a mixing device, mix evenly, and microwave for 15 minutes to obtain a protective material, and the working conditions of the microwave processor are a microwave frequency of 2450MHz and an output power of 700W;

[0030] S2: Select an optical cable and evenly coat the fiber paste on the surface of the optical cable to obtain an optical cable coated with fiber paste. The screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:1;

[0031] S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the melted protective material into liquid and coat and package it on the surface of the optical cable. The optical cable coated with the protective material can be dried to obtain a finished communication optical cable.

[0032] Reference Figure 1 , Embodiment 3

[0033] This embodiment provides a processing technology for communication optical cable, including the following steps:

[0034] S1: prepare fiber paste and protective material, the weight parts of fiber paste include 86 parts of epoxy soybean oil, 10 parts of gelling agent, 3.3 parts of styrene butadiene rubber and 0.7 parts of antioxidant, the weight parts of protective material include 79 parts of polyethylene, 14 parts of nano rubber powder, 4 parts of ultrafine magnesium oxide and 3 parts of reinforcing fiber, the reinforcing fiber includes coconut charcoal fiber and para-aramid fiber, the gelling agent selects polymer copolymer, the polymer copolymer is a hydrogenated copolymer of ethylene compound and rubber, styrene butadiene rubber is obtained in advance, the styrene butadiene rubber is poured into a crushing and grinding equipment, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain styrene butadiene rubber that passes the 200-mesh sieve, the preparation method of fiber paste: obtain epoxy soybean oil, heat the epoxy soybean oil to 80°C, then add the gelling agent and styrene butadiene rubber to stir and mix, use a microwave processor to stir under microwave reflux for 9 minutes , then add an antioxidant, continue to stir under microwave reflux for 15 minutes, stir evenly, continue heating until all the materials are melted and mixed into a liquid to obtain a fiber paste, a method for preparing ultrafine magnesium oxide: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge, wash, vacuum and dry at room temperature, burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers, a method for preparing a protective material: pour polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber into a mixing device, mix evenly, and microwave for 15 minutes to obtain a protective material, and the working conditions of the microwave processor are a microwave frequency of 2450MHz and an output power of 700W;

[0035] S2: Select an optical cable and evenly coat the fiber paste on the surface of the optical cable to obtain an optical cable coated with fiber paste. The screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:1;

[0036] S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the melted protective material into liquid and coat and package it on the surface of the optical cable. The optical cable coated with the protective material can be dried to obtain a finished communication optical cable.

[0037] Reference Figure 1 , Embodiment 4

[0038] This embodiment provides a processing technology for communication optical cable, including the following steps:

[0039] S1: prepare fiber paste and protective material, the weight parts of fiber paste include 87 parts of epoxy soybean oil, 9 parts of gelling agent, 3.5 parts of styrene butadiene rubber and 0.5 parts of antioxidant, the weight parts of protective material include 80 parts of polyethylene, 14 parts of nano rubber powder, 3 parts of ultrafine magnesium oxide and 3 parts of reinforcing fiber, the reinforcing fiber includes coconut charcoal fiber and para-aramid fiber, the gelling agent selects polymer copolymer, the polymer copolymer is a hydrogenated copolymer of ethylene compound and rubber, styrene butadiene rubber is obtained in advance, the styrene butadiene rubber is poured into a crushing and grinding equipment, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain styrene butadiene rubber that passes the 200-mesh sieve, the preparation method of fiber paste: obtain epoxy soybean oil, heat the epoxy soybean oil to 80°C, then add the gelling agent and styrene butadiene rubber to stir and mix, use a microwave processor to stir under microwave reflux for 9 minutes , then add an antioxidant, continue to stir under microwave reflux for 15 minutes, stir evenly, continue heating until all the materials are melted and mixed into a liquid to obtain a fiber paste, a method for preparing ultrafine magnesium oxide: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge, wash, vacuum and dry at room temperature, burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers, a method for preparing a protective material: pour polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber into a mixing device, mix evenly, and microwave for 15 minutes to obtain a protective material, and the working conditions of the microwave processor are a microwave frequency of 2450MHz and an output power of 700W;

[0040] S2: Select an optical cable and evenly coat the fiber paste on the surface of the optical cable to obtain an optical cable coated with fiber paste. The screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:1;

[0041] S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the melted protective material into liquid and coat and package it on the surface of the optical cable. The optical cable coated with the protective material can be dried to obtain a finished communication optical cable.

[0042] Reference Figure 1 Embodiment 5

[0043] This embodiment provides a processing technology for communication optical cable, including the following steps:

[0044] S1: prepare fiber paste and protective material, the weight parts of fiber paste include 88 parts of epoxy soybean oil, 8 parts of gelling agent, 3.8 parts of styrene butadiene rubber and 0.2 parts of antioxidant, the weight parts of protective material include 85 parts of polyethylene, 11 parts of nano rubber powder, 2 parts of ultrafine magnesium oxide and 2 parts of reinforcing fiber, the reinforcing fiber includes coconut charcoal fiber and para-aramid fiber, the gelling agent selects polymer copolymer, the polymer copolymer is a hydrogenated copolymer of ethylene compound and rubber, styrene butadiene rubber is obtained in advance, the styrene butadiene rubber is poured into a crushing and grinding equipment, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain styrene butadiene rubber that passes the 200-mesh sieve, the preparation method of fiber paste: obtain epoxy soybean oil, heat the epoxy soybean oil to 80°C, then add the gelling agent and styrene butadiene rubber to stir and mix, use a microwave processor to stir under microwave reflux for 9 minutes , then add an antioxidant, continue to stir under microwave reflux for 15 minutes, stir evenly, continue heating until all the materials are melted and mixed into a liquid to obtain a fiber paste, a method for preparing ultrafine magnesium oxide: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge, wash, vacuum and dry at room temperature, burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers, a method for preparing a protective material: pour polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber into a mixing device, mix evenly, and microwave for 15 minutes to obtain a protective material, and the working conditions of the microwave processor are a microwave frequency of 2450MHz and an output power of 700W;

[0045] S2: Select an optical cable and evenly coat the fiber paste on the surface of the optical cable to obtain an optical cable coated with fiber paste. The screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:1;

[0046] S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the melted protective material into liquid and coat and package it on the surface of the optical cable. The optical cable coated with the protective material can be dried to obtain a finished communication optical cable.

[0047] Comparing the conventional communication optical cable with the communication optical cable prepared in Examples 1 to 5, the communication optical cables prepared in Examples 1 to 5 are shown in the following table:

[0048]

[0049] It can be seen from the above table that the size and weight of the communication optical cable produced by the present invention are reduced, no delamination phenomenon occurs, and implementation 2 is the best implementation example.

[0050] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A processing technology for communication optical cable, characterized in that: The following steps are involved: S1: preparing a fiber paste and a protective material, wherein the fiber paste comprises 70 to 90 parts by weight of epoxy soybean oil, 2 to 10 parts of a gelling agent, 1.0 to 4.0 parts of styrene-butadiene rubber and 0.2 to 1.0 parts of an antioxidant, and the protective material comprises 75 to 85 parts by weight of polyethylene, 10 to 15 parts of nano rubber powder, 1 to 5 parts of ultrafine magnesium oxide and 1 to 5 parts of reinforcing fiber, wherein the reinforcing fiber comprises coconut charcoal fiber and para-aramid fiber; S2: Select an optical cable and evenly apply the fiber paste on the surface of the optical cable to obtain an optical cable coated with the fiber paste; S3: Pour the protective material into a mixing extruder for stirring, mixing and heating. The mixing extruder extrude the protective material melted into liquid and coat and package it on the surface of the optical cable.

2. A processing technology for communication optical cable according to claim 1, characterized in that: In S1, the gelling agent is a high molecular copolymer, which is a hydrogenated copolymer of ethylene compounds and rubber.

3. A processing technology for communication optical cable according to claim 1, characterized in that: In S1, styrene butadiene rubber is obtained in advance, poured into a crushing and grinding device, first crushed, and then ground into powder, the crushed styrene butadiene rubber is screened through a 200-mesh sieve, and the styrene butadiene rubber that does not pass the screening is ground again to obtain the styrene butadiene rubber that passes the 200-mesh sieve.

4. A processing technology for communication optical cable according to claim 1, characterized in that: In S1, the preparation method of the fiber paste is as follows: obtain epoxy soybean oil, heat the epoxy soybean oil to 80°C, then add a gelling agent and styrene-butadiene rubber to stir and mix, use a microwave processor to reflux and stir for 9 minutes, then add an antioxidant, continue to reflux and stir for 15 minutes, stir well and continue to heat until all the materials are melted and mixed into a liquid to obtain a fiber paste.

5. The processing technology of a communication optical cable according to claim 1, characterized in that: In S1, the preparation method of ultrafine magnesium oxide is as follows: obtain a soluble magnesium salt, add a surfactant and sodium oxalate, mix the soluble magnesium salt, the surfactant and the sodium oxalate evenly to obtain a mixture, pour the mixture into an autoclave for hydrothermal reaction, take out the precursor precipitate, centrifuge wash, vacuum dry at room temperature, and burn the dried precursor in a muffle furnace to obtain ultrafine magnesium oxide.

6. A processing technology for communication optical cable according to claim 1, characterized in that: In S1, the ratio of coconut charcoal fiber to para-aramid fiber in the reinforcing fiber is controlled at 2:1, and both coconut charcoal fiber and para-aramid fiber are short fibers.

7. The processing technology of a communication optical cable according to claim 1, characterized in that: In S1, the preparation method of the protective material is as follows: polyethylene, nano rubber powder, ultrafine magnesium oxide and reinforcing fiber are poured into a mixing device and mixed evenly, and microwaved for 15 minutes to obtain the protective material.

8. A processing technology for communication optical cable according to claim 7, characterized in that: In S1, the working conditions of the microwave processor are a microwave frequency of 2450 MHz and an output power of 700 W.

9. The processing technology of a communication optical cable according to claim 1, characterized in that: In S3, the screw length-diameter ratio of the mixing extruder is 20:1-25:1, the clearance between the screw and the barrel is 0.14-0.18 mm, and the compression ratio is 4:1 or 3.5:

1.

10. The processing technology of a communication optical cable according to claim 1, characterized in that: In S3, the optical cable coated with the protective material is dried to obtain a finished communication optical cable.