High-frequency response composite single crystal thin film, preparation method thereof and modulator

By adopting a composite single-crystal thin film structure in a silicon-based thin film lithium niobate modulator, combining high-dielectric constant and low-dielectric constant materials, the problems of microwave loss and process maturity are solved, and high-frequency response and high-efficiency electro-optical modulation are achieved. .

CN118981122APending Publication Date: 2024-11-19JINAN JINGZHENG ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044756.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing silicon-based thin-film lithium niobate modulators lead to an increase in microwave losses after the electrode spacing is reduced, affecting device performance, and the maturity of single crystal quartz substrate process is low, limiting large-scale production.

Method used

Using a composite single crystal thin film structure, a high-dielectric constant material layer, a low-dielectric constant material layer and an electro-optical crystal thin film layer are combined, and an isolation layer is set between the low-dielectric constant material layer and the electro-optical crystal thin film layer, and an ion implantation is carried out. The composite single crystal film is formed with annealing treatment, which is used in the modulator to reduce microwave losses and improve high frequency response.

Benefits of technology

It realizes high-frequency response characteristics and ultra-high modulation bandwidth, reduces the half-wave voltage length product, optimizes thermal management, improves electro-optical modulation efficiency, and has low power consumption and high compatibility, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118981122A_ABST
    Figure CN118981122A_ABST
Patent Text Reader

Abstract

The invention discloses a high-frequency response composite single crystal thin film, a preparation method thereof and a modulator, and the composite single crystal thin film at least comprises a high-dielectric-constant material layer, a low-dielectric-constant material layer and an electro-optical crystal thin film layer from bottom to top in sequence. An isolating layer is further arranged in the low-dielectric-constant material layer and the electro-optical crystal thin film layer. The thin film is applied to a modulator by considering the technological maturity of a silicon material and the high-frequency response characteristic of a low-dielectric-constant material. The preparation method comprises the following steps: bonding the high-dielectric-constant material layer and the low-dielectric-constant material layer to obtain a first bonding body; performing ion implantation and bonding stripping on the electro-optical crystal material to obtain a composite single crystal thin film, or depositing an isolation layer on a first bonding body to be bonded with the electro-optical crystal thin film layer; and generating an oxide layer on the other high-dielectric-constant material layer, bonding the oxide layer with the electro-optical crystal thin film layer, then bonding the oxide layer with the first bonding body isolation layer, and corroding to obtain the composite single crystal thin film. The preparation method has the advantages of small stress, short period and high compatibility with the existing process, and is beneficial to large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a composite single crystal film with high frequency response, a preparation method thereof, and a modulator. Background Art

[0002] At present, the processing technology of silicon materials is very mature, and it is also a semiconductor material with more industrial applications. Therefore, silicon materials have been widely used in electronic components. Since silicon materials themselves have a centrosymmetric crystal structure, silicon has no linear electro-optical effect. Therefore, silicon materials cannot be directly used to prepare high-performance electro-optical materials. Lithium niobate has become the first choice for preparing electro-optical materials and modulators due to its high electro-optic coefficient, wide transmission window and low optical loss in the communication band. Compared with the traditional lithium niobate platform, the silicon-based thin-film lithium niobate material provides significant voltage-bandwidth performance while retaining the excellent physical properties of lithium niobate bulk materials, such as linear response, high extinction ratio, and high optical power handling capability.

[0003] For silicon-based thin-film lithium niobate modulators, benefiting from the strong light field confinement effect of the thin-film ridge waveguide structure, the electrode spacing can be reduced to a few micrometers, thereby enhancing the electro-optical interaction and improving the electro-optical modulation efficiency. However, the reduction in electrode spacing will lead to increased microwave loss, thereby increasing the power consumption of the device and affecting the device's performance such as sensitivity and noise. The use of a T-type electrode structure can reduce microwave loss without increasing the electrode spacing, that is, without reducing the electro-optical modulation efficiency. However, the slow wave effect caused by the T-type electrode structure will increase the effective refractive index of microwaves, which will make it difficult to achieve speed matching between microwaves and light waves. Using single crystal quartz as a substrate can reduce the effective refractive index of microwaves and show better high-frequency response. However, since the process maturity of quartz-based materials is much lower than that of silicon materials, it brings a series of yield and cost issues, and has low compatibility with existing processes, which is not conducive to large-scale production. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and to provide a composite single crystal film with high frequency response and a preparation method thereof, and a modulator.

[0005] To achieve the above purpose, the technical solution provided by the present invention is as follows:

[0006] A composite single crystal film, which comprises at least: a high dielectric constant material layer, a low dielectric constant material layer, and an electro-optical crystal film layer in order from bottom to top.

[0007] The composite single crystal film is further provided with an isolation layer between the low dielectric constant material layer and the electro-optical crystal film layer.

[0008] The high dielectric constant material layer is silicon, diamond, silicon carbide, silicon nitride, gallium arsenide or indium phosphide, and the thickness of the high dielectric constant material layer is 100 μm to 1 mm. The dielectric constant of the low dielectric constant layer is not greater than 4.5, and the low dielectric constant material layer is HPFS ( Fused Silica Wafer, Ultra-high purity: 100%SiO2, dielectric constant 3.79, loss tangent 2*10 -5 ), FSG (fluorine-doped silica glass) or PI (polyimide), the thickness of the low dielectric constant material layer is 1μm to 100μm, and the roughness of the low dielectric constant material layer is not greater than 0.5nm.

[0009] The isolation layer is made of aluminum oxide, aluminum nitride, silicon carbide, silicon dioxide or silicon nitride, the thickness of the isolation layer is 50nm-20μm, and the roughness of the isolation layer is not greater than 0.5nm.

[0010] The electro-optical crystal thin film layer is lithium niobate crystal, lithium tantalate crystal, gallium arsenide, silicon, ceramic, lithium tetraborate, gallium arsenide, potassium titanyl phosphate, rubidium titanyl phosphate crystal or quartz, and the thickness of the electro-optical crystal thin film layer is 50nm to 20μm.

[0011] A modulator comprises the composite single crystal film, wherein the electro-optical crystal film layer of the composite single crystal film is etched to form a thin film optical waveguide layer, and an electrode for modulating optical signals is arranged above the thin film optical waveguide layer.

[0012] A method for preparing a composite single crystal thin film, the method is used to prepare the composite single crystal thin film, the method comprises the following steps:

[0013] (1) bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body;

[0014] (2) performing ion implantation on the electro-optical crystal material and bonding it with the low dielectric constant material layer to obtain a second bonded body;

[0015] (3) The second bonded body is subjected to primary annealing and peeling, secondary annealing to eliminate implantation damage, and thinning in sequence to obtain a composite single crystal thin film.

[0016] A method for preparing a composite single crystal thin film, the method is used to prepare the composite single crystal thin film, the method comprises the following steps:

[0017] (1) bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body;

[0018] (2) depositing an isolation layer on the surface of the low dielectric constant material layer of the first bonding body;

[0019] (3) performing ion implantation on the electro-optical crystal material and bonding it with the isolation layer to obtain a second bonded body;

[0020] (4) The second bonded body is subjected to primary annealing for stripping, secondary annealing for eliminating implantation damage, and thinning in sequence to obtain a composite single crystal thin film.

[0021] A method for preparing a composite single crystal thin film, the method is used to prepare the composite single crystal thin film, the method comprises the following steps:

[0022] (1) bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body;

[0023] (2) depositing an isolation layer on the surface of the low dielectric constant material layer of the first bonding body;

[0024] (3) thermally oxidizing the surface of another high dielectric constant material layer to form an oxide layer;

[0025] (4) performing ion implantation on the electro-optical crystal material and bonding it with the oxide layer in (3) to obtain a second bonded body;

[0026] (5) performing a primary annealing and peeling, a secondary annealing to eliminate implantation damage, and thinning the second bonding body in sequence, and bonding the second bonding body with an isolation layer to obtain a third bonding body;

[0027] (6) The third bonding body is placed in an etching solution to remove the high dielectric constant material layer and silicon dioxide of the second bonding body to obtain a composite single crystal thin film.

[0028] In the method for preparing the composite single crystal film, the high dielectric constant material layer is silicon, diamond, silicon carbide, silicon nitride, gallium arsenide or indium phosphide.

[0029] The method for preparing the composite single crystal thin film, the dielectric constant of the low dielectric constant layer is not greater than 4.5, and the low dielectric constant material layer is HPFS ( Fused Silica Wafer, Ultra-high purity: 100%SiO2, dielectric constant 3.79, loss tangent 2*10 -5 ), FSG (fluorine-doped silica glass) or PI (polyimide).

[0030] The preparation method of the composite single crystal film, the electro-optical crystal material is lithium niobate crystal, lithium tantalate crystal, gallium arsenide, silicon, ceramic, lithium tetraborate, gallium arsenide, potassium titanyl phosphate, rubidium titanyl phosphate crystal or quartz.

[0031] In the method for preparing the composite single crystal thin film, the isolation layer is aluminum oxide, aluminum nitride, silicon carbide, silicon dioxide or silicon nitride.

[0032] The method for preparing the composite single crystal thin film, wherein the method for depositing the isolation layer is sputtering, low-pressure chemical vapor deposition, plasma enhanced chemical vapor deposition or chemical vapor deposition.

[0033] The method for preparing the composite single crystal thin film, wherein the ions are helium ions, the ion implantation energy is set to 30 KeV to 5 MeV, and the dose is set to 1×10 15 ions / cm 2 ~1×10 17 ions / cm 2 .

[0034] In the method for preparing the composite single crystal thin film, the temperature for the first annealing and peeling of the second bonding body is 150° C. to 400° C., the temperature for the second annealing of the second bonding body is 300° C. to 600° C., and the time is 0.5 h to 48 h.

[0035] The method for preparing the composite single crystal film, wherein the thinning method is chemical mechanical polishing or grinding.

[0036] In step (3), the oxide layer is silicon dioxide or aluminum oxide, the thickness of the oxide layer is 50 nm to 20 μm, and the roughness is not greater than 0.5 nm.

[0037] In the method for preparing the composite single crystal thin film, in step (6), the etching solution is TMAH etching solution or HF solution, wherein the HF solution is a pure HF solution or a HF:pure water mixture with a concentration of not less than 1:1000.

[0038] Beneficial effects:

[0039] The present application provides a high-frequency responsive composite single crystal film and a preparation method thereof, and a modulator, wherein the composite single crystal film comprises, from bottom to top, a high dielectric constant material layer, a low dielectric constant material layer, and an electro-optical crystal film layer. The composite single crystal film of the present invention uses a low dielectric material placed between the electro-optical crystal film layer and the high dielectric constant material layer, and utilizes its low dielectric constant and low loss tangent value to enable the composite single crystal film to have better high-frequency response characteristics.

[0040] An isolation layer is also provided between the low dielectric constant material layer and the electro-optical crystal film layer to form a composite single crystal film. The composite single crystal film layer is applied to the modulator to solve the microwave and light wave speed adaptation problem caused by the slow wave effect caused by the T-type electrode structure of the lithium niobate thin film modulator. The modulator prepared using this composite single crystal film can have both ultra-high modulation bandwidth and ultra-low half-wave voltage. By using a composite film with alternating high dielectric constant material layers and low dielectric constant material layers in the electro-optic modulator, the high dielectric constant layer can enhance the local electric field strength, while the low dielectric constant layer helps to reduce the shielding effect of the electric field. This design can make the electric field more concentratedly distributed on the light wave propagation path, which can enhance the electric field strength and its overlap with the light field, thereby improving the modulation efficiency. For example, a thin-film lithium niobate electro-optic modulator with a high dielectric constant cladding achieves a lower half-wave voltage-length product and a wider 3dB EO bandwidth by increasing the electric field strength in the waveguide. Materials with different dielectric constants have material interfaces, and the optical reflection effect at the interface helps to reflect the leaked light field, better control the light field in the thin film layer, and reduce optical losses. Layers with different dielectric constants have different thermal expansion coefficients, and this difference can be used to optimize the thermal management of the device and reduce the impact of thermal effects on device performance.

[0041] The preparation method includes bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body, ion implanting and bonding an electro-optical crystal material to obtain a composite single crystal film, or depositing an isolation layer on the first bonding body and bonding it to the electro-optical crystal film layer; and also includes bonding the oxide layer on another high dielectric constant material layer to the electro-optical crystal film layer and then bonding it to the isolation layer of the first bonding body, etching, and obtaining a composite single crystal film. It can be seen from the above technical solution that the film preparation method has the advantages of low stress, short preparation cycle, high compatibility with existing processes, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0043] Figure 1 is a schematic diagram of the structure of a composite single crystal thin film provided in an embodiment of the present application;

[0044] Figure 2 is a schematic diagram of the structure of a composite single crystal thin film provided in an embodiment of the present application;

[0045] Figure 3 It is a structural schematic diagram of a method for preparing a composite single crystal thin film provided in an embodiment of the present application;

[0046] Figure 4 It is a structural schematic diagram of a method for preparing a composite single crystal thin film provided in an embodiment of the present application;

[0047] Figure 5 It is a structural schematic diagram of a method for preparing a composite single crystal thin film provided in an embodiment of the present application.

[0048] Among them, 110-high dielectric constant material layer; 120-low dielectric constant material layer; 130-isolation layer; 1401-electro-optical crystal film layer; 1402-separation layer; 1403-residue material layer; 140-electro-optical crystal material; 150-oxide layer. DETAILED DESCRIPTION

[0049] The present invention is further illustrated below in conjunction with specific embodiments. The embodiments are implemented based on the technical solutions of the present invention. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0050] Embodiment 1 (smart-cut method)

[0051] (1) Prepare a single crystal silicon substrate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface, and also prepare a HPFS wafer with a size of 4 inches, a thickness of 0.5 mm and a smooth surface. After cleaning the process surfaces of the silicon substrate wafer and the HPFS wafer respectively, bond the two wafer process surfaces using room temperature bonding technology to obtain a first bonded body. Then put the bonded body into an oven and anneal at 100°C for 48 hours. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to thin the HPFS thickness to 100μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2mm HPFS portion of the edge of the first bonded body.

[0052] (2) The HPFS surface of the first bonded body is cleaned and a layer of silicon dioxide is deposited as an isolation layer (130). The silicon dioxide is deposited by low pressure chemical vapor deposition and the deposition thickness is 50 nm. The first bonded body after the silicon dioxide deposition is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss. The HPFS surface roughness is not greater than 0.5 nm, and the silicon dioxide roughness is processed to 0.2 nm by chemical mechanical polishing.

[0053] (3) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 400 KeV and the dose was set to 1×10 17 ions / cm 2A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed, and bonded to the isolation layer (130) in step (2) to obtain a second bonded body.

[0054] (4) Then, the second bonded body is annealed at 400° C. in an oven to peel off the lithium niobate wafer to form a lithium niobate film, until the thin film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of the lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 300° C. for 48 hours to eliminate the injection damage, and finally, the lithium niobate film is polished and thinned to 900 nm to obtain a composite single crystal film. The composite single crystal film structure is Figure 1 As shown, the composite single crystal thin film preparation method is as follows Figure 3 As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), silicon dioxide forms an isolation layer (130), the lithium niobate wafer forms an electro-optical crystal material (140), and the lithium niobate film forms an electro-optical crystal film layer (1401).

[0055] Embodiment 2 (smart-cut method)

[0056] (1) Prepare a 4-inch, 1mm thick, smooth single crystal silicon substrate wafer, and also prepare a 4-inch, 0.5mm thick, smooth HPFS wafer. Clean the process surfaces of the silicon substrate wafer and the HPFS wafer respectively, and bond the two wafer process surfaces using room temperature bonding technology to obtain a first bonded body. Then place the bonded body in an oven and anneal at 100°C for 48 hours. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to reduce the HPFS thickness to 20μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2mm HPFS portion of the edge of the first bonded body.

[0057] (2) The HPFS surface of the first bonded body is cleaned and a layer of silicon dioxide is deposited as an isolation layer (130). The silicon dioxide is deposited by low pressure chemical vapor deposition and the deposition thickness is 20 μm. The first bonded body after the silicon dioxide deposition is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss. The HPFS surface roughness is not greater than 0.5 nm, and the silicon dioxide roughness is processed to 0.2 nm by chemical mechanical polishing.

[0058] (3) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 400 KeV and the dose was set to 1×10 17 ions / cm 2 A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed, and bonded to the isolation layer (130) in step (2) to obtain a second bonded body.

[0059] (4) Then, the second bonded body is annealed at 150°C in an oven to achieve lithium niobate wafer peeling to form a lithium niobate film, until the film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 500°C for 24 hours to eliminate the injection damage, and finally the lithium niobate film is polished and thinned to 50nm to obtain a composite single crystal film. The composite single crystal film structure is Figure 1 As shown, the composite single crystal thin film preparation method is as follows Figure 3 As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), silicon dioxide forms an isolation layer (130), the lithium niobate wafer forms an electro-optical crystal material (140), and the lithium niobate film forms an electro-optical crystal film layer (1401).

[0060] Example 3 (smart-cut method + film transfer method preparation)

[0061] (1) Prepare a 4-inch, 100 μm thick, smooth single crystal silicon substrate wafer, and also prepare a 4-inch, 0.5 mm thick, smooth HPFS wafer. After cleaning the process surfaces of the silicon substrate wafer and the HPFS wafer, bond the two wafer process surfaces using room temperature bonding technology to obtain a first bonded body. Then place the bonded body in an oven and anneal at 400°C for 0.5 h. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to reduce the HPFS thickness to 20 μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2 mm HPFS portion of the edge of the first bonded body.

[0062] (2) The HPFS surface of the first bond body is cleaned and a layer of silicon dioxide is deposited as an isolation layer (130). The silicon dioxide is deposited by plasma enhanced chemical vapor deposition with a deposition thickness of 5 μm. The first bond body after the silicon dioxide deposition is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss. The HPFS surface roughness is not greater than 0.5 nm, and the silicon dioxide roughness is treated to 0.3 nm by chemical mechanical polishing.

[0063] (3) A single crystal silicon substrate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface is prepared, and is cleaned and subjected to a thermal oxidation process to form a 2 μm silicon dioxide layer on its surface.

[0064] (4) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 100 KeV and the dose was set to 1×10 17 ions / cm 2 A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed. The ion-implanted lithium niobate thin film layer is bonded to the silicon substrate wafer silicon dioxide obtained in step (3) by plasma bonding to obtain a second bonded body.

[0065] (5) The bonded body is then annealed at 400°C to achieve lithium niobate wafer peeling to form a lithium niobate film, until the film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 600°C for 0.5h to eliminate injection damage. Finally, the lithium niobate film is polished and thinned to 100nm to obtain a nano-scale lithium niobate film structure. The isolation layer (130) of the first bonded body and the electro-optical crystal film layer (1401) of the second bonded body are cleaned respectively, and they are bonded by plasma bonding to obtain a third bonded body.

[0066] (6) Then the bonded body is placed in an oven device for annealing at 600°C for 0.5h, and the third bonded body is thinned, with the thinned surface being the high dielectric constant material layer of the second bonded body. The silicon high dielectric constant material layer of the second bonded body is thinned to 5μm by grinding. Then the thinned third bonded body is placed in TMAH silicon etching solution at 60°C for 24h and HF etching solution at room temperature for 3h, respectively, to remove the high dielectric constant material layer and silicon dioxide of the second bonded body, and obtain a composite single crystal film. The composite single crystal film structure is Figure 1 As shown, the composite single crystal thin film preparation method is as follows Figure 4As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), silicon dioxide forms an isolation layer (130), the lithium niobate wafer forms an electro-optical crystal material (140), the lithium niobate film forms an electro-optical crystal film layer (1401), and silicon dioxide is an oxide layer (150).

[0067] Example 4 (smart-cut method + film transfer method preparation)

[0068] (1) Prepare a 4-inch, 0.525mm thick, smooth single crystal silicon substrate wafer, and a 4-inch, 0.5mm thick, smooth HPFS wafer. Clean the process surfaces of the silicon substrate wafer and the HPFS wafer respectively, and bond the process surfaces of the two wafers using room temperature bonding technology to obtain a first bonded body. Then place the bonded body in an oven and anneal at 400°C for 0.5h. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to reduce the HPFS thickness to 1μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2mm HPFS portion of the edge of the first bonded body.

[0069] (2) The HPFS surface of the first bond body is cleaned and a layer of silicon dioxide is deposited as an isolation layer (130). The silicon dioxide is deposited by plasma enhanced chemical vapor deposition with a deposition thickness of 20 μm. The first bond body after the silicon dioxide deposition is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss. The HPFS surface roughness is not greater than 0.5 nm, and the silicon dioxide roughness is treated to 0.3 nm by chemical mechanical polishing.

[0070] (3) A single crystal silicon substrate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface is prepared, and is cleaned and subjected to a thermal oxidation process to form a 20 μm layer of silicon dioxide on its surface.

[0071] (4) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 5 MeV and the dose was set to 1×10 15 ions / cm 2 A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed. The ion-implanted lithium niobate thin film layer is bonded to the silicon substrate wafer silicon dioxide obtained in step (3) by plasma bonding to obtain a second bonded body.

[0072] (5) The bonded body is then annealed at 400°C to achieve lithium niobate wafer peeling to form a lithium niobate film, until the film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 600°C for 0.5h to eliminate injection damage. Finally, the lithium niobate film is polished and thinned to 100nm to obtain a nano-scale lithium niobate film structure. The isolation layer (130) of the first bonded body and the electro-optical crystal film layer (1401) of the second bonded body are cleaned respectively, and they are bonded by plasma bonding to obtain a third bonded body.

[0073] (6) Then the bonded body is placed in an oven and annealed at 100°C for 48 hours, and the third bonded body is thinned, with the thinned surface being the high dielectric constant material layer of the second bonded body. The high dielectric constant material layer of the second bonded body is thinned to 1 μm by grinding. Then the thinned third bonded body is placed in a TMAH silicon etching solution at 60°C for 12 hours and in an HF etching solution at room temperature for 3 hours, respectively, to remove the high dielectric constant material layer and silicon dioxide of the second bonded body, and obtain a composite single crystal film. The composite single crystal film structure is Figure 1 As shown, the composite single crystal thin film preparation method is as follows Figure 4 As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), silicon dioxide forms an isolation layer (130), the lithium niobate wafer forms an electro-optical crystal material (140), the lithium niobate film forms an electro-optical crystal film layer (1401), and silicon dioxide is an oxide layer (150).

[0074] Example 5 (smart-cut method + film transfer method preparation)

[0075] (1) Prepare a 4-inch, 100μm thick, smooth single crystal silicon substrate wafer, and also prepare a 4-inch, 0.5mm thick, smooth HPFS wafer. Clean the process surfaces of the silicon substrate wafer and the HPFS wafer respectively, and bond the process surfaces of the two wafers using room temperature bonding technology to obtain a first bonded body. Then, place the bonded body in an oven and anneal at 400°C for 0.5h. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to reduce the HPFS thickness to 20μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2mm HPFS portion of the edge of the first bonded body.

[0076] (2) The HPFS surface of the first bond body is cleaned and a layer of silicon dioxide is deposited as an isolation layer (130). The silicon dioxide is deposited by plasma enhanced chemical vapor deposition with a deposition thickness of 5 μm. The first bond body after the silicon dioxide deposition is annealed to eliminate impurity ions in the deposited silicon dioxide layer to reduce absorption loss. The HPFS surface roughness is not greater than 0.5 nm, and the silicon dioxide roughness is treated to 0.3 nm by chemical mechanical polishing.

[0077] (3) A single crystal silicon substrate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface is prepared, and is cleaned and subjected to a thermal oxidation process to form a 50 nm layer of silicon dioxide on its surface.

[0078] (4) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 100 KeV and the dose was set to 1×10 17 ions / cm 2 A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed. The ion-implanted lithium niobate thin film layer is bonded to the silicon substrate wafer silicon dioxide obtained in step (3) by plasma bonding to obtain a second bonded body.

[0079] (5) The bonded body is then annealed at 400°C to achieve lithium niobate wafer peeling to form a lithium niobate film, until the film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 600°C for 0.5h to eliminate injection damage. Finally, the lithium niobate film is polished and thinned to 100nm to obtain a nano-scale lithium niobate film structure. The isolation layer (130) of the first bonded body and the electro-optical crystal film layer (1401) of the second bonded body are cleaned respectively, and they are bonded by plasma bonding to obtain a third bonded body.

[0080] (6) Then the bonded body is placed in an oven and annealed at 600°C for 0.5h, and the third bonded body is thinned, with the thinned surface being the high dielectric constant material layer of the second bonded body. The high dielectric constant material layer of the second bonded body is thinned to 100μm by grinding. Then the thinned third bonded body is placed in TMAH silicon etching solution at 60°C for 24h and HF etching solution at room temperature for 3h, respectively, to remove the high dielectric constant material layer and silicon dioxide of the second bonded body, and obtain a composite single crystal film. The composite single crystal film structure is Figure 1 As shown, the composite single crystal thin film preparation method is as follows Figure 4As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), silicon dioxide forms an isolation layer (130), the lithium niobate wafer forms an electro-optical crystal material (140), the lithium niobate film forms an electro-optical crystal film layer (1401), and silicon dioxide is an oxide layer (150).

[0081] Example 6 (smart-cut method + no isolation layer)

[0082] (1) Prepare a 4-inch, 0.525mm thick, smooth single crystal silicon substrate wafer, and also prepare a 4-inch, 0.5mm thick, smooth HPFS wafer. Clean the process surfaces of the silicon substrate wafer and the HPFS wafer respectively, and bond the process surfaces of the two wafers using room temperature bonding technology to obtain a first bonded body. Then place the bonded body in an oven and anneal at 100°C for 48 hours. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to reduce the HPFS thickness to 20μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2mm HPFS portion of the edge of the first bonded body.

[0083] (2) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 400 KeV and the dose was set to 1×10 17 ions / cm 2 A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed and bonded to the HPFS surface of the first bonding body to obtain a second bonding body.

[0084] (3) Then, the second bonded body is annealed in an oven at 150° C. to achieve lithium niobate wafer peeling to form a lithium niobate film, until the thin film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 500° C. for 24 hours to eliminate the injection damage, and finally, the lithium niobate film is polished and thinned to 900 nm to obtain a composite single crystal film. The composite single crystal film structure is Figure 2 As shown, the composite single crystal thin film preparation method is as follows Figure 5 As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), the lithium niobate wafer forms an electro-optical crystal material (140), and the lithium niobate film forms an electro-optical crystal film layer (1401).

[0085] Example 7 (smart-cut method + no isolation layer)

[0086] (1) Prepare a single crystal silicon substrate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface, and also prepare a HPFS wafer with a size of 4 inches, a thickness of 0.5 mm and a smooth surface. After cleaning the process surfaces of the silicon substrate wafer and the HPFS wafer respectively, bond the two wafer process surfaces using room temperature bonding technology to obtain a first bonded body. Then put the bonded body into an oven and anneal at 100°C for 48 hours. Thin and grind the HPFS surface of the annealed first bonded body, and use chemical mechanical polishing to thin the HPFS thickness to 100μm. If there is an unbonded area on the edge of the first bonded body due to wafer chamfering, a grinding process is required to remove the 1-2mm HPFS portion of the edge of the first bonded body.

[0087] (2) A lithium niobate wafer with a size of 4 inches, a thickness of 0.525 mm and a smooth surface was prepared, and helium ions (He+) were implanted into the lithium niobate wafer by ion implantation. The implantation energy of the helium ions was set to 400 KeV and the dose was set to 1×10 17 ions / cm 2 A lithium niobate wafer having a three-layer structure of an electro-optical crystal thin film layer (1401), a separation layer (1402) and a residual material layer (1403) is formed and bonded to the HPFS surface of the first bonding body to obtain a second bonding body.

[0088] (3) Then, the second bonded body is annealed in an oven at 150° C. to achieve lithium niobate wafer peeling to form a lithium niobate film, until the film layer of the lithium niobate film wafer is separated from the bonded body to form a top layer of lithium niobate film, and then the obtained second bonded body structure is placed in an oven and annealed at 500° C. for 24 hours to eliminate the injection damage, and finally, the lithium niobate film is polished and thinned to 20 μm to obtain a composite single crystal film. The composite single crystal film structure is Figure 2 As shown, the composite single crystal thin film preparation method is as follows Figure 5 As shown in the structural schematic diagram, in this embodiment, the single crystal silicon substrate wafer forms a high dielectric constant material layer (110), the HPFS wafer forms a low dielectric constant material layer (120), the lithium niobate wafer forms an electro-optical crystal material (140), and the lithium niobate film forms an electro-optical crystal film layer (1401).

[0089] The above specific implementation methods further illustrate the purpose, technical solutions and beneficial effects of the present application in detail. It should be understood that the above are only specific implementation methods of the present application and are not used to limit the protection scope of the present application. Any modifications, equivalent substitutions, improvements, etc. made on the basis of the technical solutions of the present application should be included in the protection scope of the present application.

Claims

1. A composite single crystal thin film, characterized in that: The composite single crystal film comprises at least: a high dielectric constant material layer, a low dielectric constant material layer, and an electro-optical crystal film layer from bottom to top.

2. The composite single crystal thin film according to claim 1, characterized in that: The composite single crystal film is further provided with an isolation layer between the low dielectric constant material layer and the electro-optical crystal film layer.

3. The composite single crystal thin film according to claim 1 or 2, characterized in that: The high dielectric constant material layer is silicon, diamond, silicon carbide, silicon nitride, gallium arsenide or indium phosphide, and the high dielectric constant material layer has a thickness of 100 μm to 1 mm.

4. The composite single crystal thin film according to claim 1 or 2, characterized in that: The dielectric constant of the low dielectric constant layer is not greater than 4.5, the low dielectric constant material layer is HPFS, FSG or PI, the thickness of the low dielectric constant material layer is 1 μm to 100 μm, and the roughness of the low dielectric constant material layer is not greater than 0.5 nm.

5. The composite single crystal thin film according to claim 2, characterized in that: The isolation layer is made of aluminum oxide, aluminum nitride, silicon carbide, silicon dioxide or silicon nitride, the thickness of the isolation layer is 50nm-20μm, and the roughness of the isolation layer is not greater than 0.5nm.

6. The composite single crystal thin film according to claim 1 or 2, characterized in that: The electro-optical crystal thin film layer is lithium niobate crystal, lithium tantalate crystal, gallium arsenide, silicon, ceramic, lithium tetraborate, gallium arsenide, potassium titanyl phosphate, rubidium titanyl phosphate crystal or quartz, and the thickness of the electro-optical crystal thin film layer is 50nm to 20μm.

7. A modulator, characterized in that: It comprises the composite single crystal thin film as described in any one of claims 1 to 6.

8. The modulator according to claim 7, characterized in that The electro-optical crystal thin film layer of the composite single crystal thin film is etched to form a thin film optical waveguide layer, and an electrode for modulating optical signals is also arranged above the thin film optical waveguide layer.

9. A method for preparing a composite single crystal thin film, characterized in that: The preparation method is used to prepare the composite single crystal thin film according to claim 1, and the preparation method comprises the following steps: (1) bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body; (2) performing ion implantation on the electro-optical crystal material and bonding it with the low dielectric constant material layer to obtain a second bonded body; (3) Annealing, peeling and thinning the second bonded body to obtain a composite single crystal thin film.

10. A method for preparing a composite single crystal thin film, characterized in that: The preparation method is used to prepare the composite single crystal thin film according to claim 2, and the preparation method comprises the following steps: (1) bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body; (2) depositing an isolation layer on the surface of the low dielectric constant material layer of the first bonding body; (3) performing ion implantation on the electro-optical crystal material and bonding it with the isolation layer to obtain a second bonded body; (4) Annealing, peeling and thinning the second bonded body to obtain a composite single crystal thin film.

11. A method for preparing a composite single crystal thin film, characterized in that: The preparation method is used to prepare the composite single crystal thin film according to claim 2, and the preparation method comprises the following steps: (1) bonding a high dielectric constant material layer and a low dielectric constant material layer to obtain a first bonding body; (2) depositing an isolation layer on the surface of the low dielectric constant material layer of the first bonding body; (3) thermally oxidizing the surface of another high dielectric constant material layer to form an oxide layer; (4) performing ion implantation on the electro-optical crystal material and bonding it with the oxide layer in (3) to obtain a second bonded body; (5) annealing, peeling and thinning the second bonding body, and bonding it with an isolation layer to obtain a third bonding body; (6) The third bonding body is placed in an etching solution to remove the high dielectric constant material layer and silicon dioxide of the second bonding body to obtain a composite single crystal thin film.

12. The method for preparing a composite single crystal thin film according to claim 11, wherein in step (3), the oxide layer is silicon dioxide or aluminum oxide, the thickness of the oxide layer is 50 nm to 20 μm, and the roughness is not greater than 0.5 nm.

13. The method for preparing a composite single crystal thin film according to claim 11, wherein in step (6), the etching solution is TMAH etching solution or HF solution, wherein the HF solution is pure HF solution or a mixture of HF and pure water with a concentration of not less than 1:1000.