Silicon carbide epitaxial growth method for prolonging minority carrier lifetime and silicon carbide epitaxial wafer

By carburizing and polishing during the epitaxial growth of silicon carbide, the problem of the short life of a few carriers in the silicon carbide epitaxial sheet is solved, and the performance of SiC IGBT devices is significantly improved.

CN118983215AInactive Publication Date: 2024-11-19HEBEI POSHING ELECTRONICS TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411471660.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The lifespan of minority carriers in existing silicon carbide epitaxial sheets is too short, resulting in limited performance of SiC IGBT devices, and it is difficult for existing processes to effectively regulate the lifespan of minority.

Method used

During the epitaxial growth of silicon carbide, carburizing treatment is performed after the drift layer is grown, and chemical mechanical polishing technology is used to remove the carbon-rich layer on the surface, reducing the carbon vacancy density and minority carrier composite center of the epitaxial layer.

Benefits of technology

It significantly improves the minority carrier life and surface crystallization quality of the silicon carbide epitaxial sheet, and improves the performance of SiC IGBT devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983215A_ABST
    Figure CN118983215A_ABST
Patent Text Reader

Abstract

The invention provides a silicon carbide epitaxial growth method for prolonging minority carrier lifetime and a silicon carbide epitaxial wafer. The method comprises the following steps: placing a silicon carbide substrate in a reaction cavity of silicon carbide epitaxial equipment, and sequentially carrying out etching, buffer layer growth and drift layer growth on the silicon carbide substrate; after the drift layer with the first thickness is obtained, carbon source gas is introduced into the reaction cavity, the temperature of the reaction cavity is increased to a first preset temperature, carburization is conducted on the drift layer, and an initial silicon carbide epitaxial wafer is obtained; and polishing the silicon-containing surface of the initial silicon carbide epitaxial wafer by adopting a chemical mechanical polishing technology to obtain the silicon carbide epitaxial wafer containing the drift layer with the target thickness, and the first thickness is greater than the target thickness. The service life of minority carriers of the silicon carbide epitaxial wafer is greatly prolonged, and the surface crystallization quality of the silicon carbide epitaxial wafer is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of silicon carbide epitaxial wafers, and in particular to a silicon carbide epitaxial growth method and a silicon carbide epitaxial wafer for improving minority carrier lifetime. Background Art

[0002] Silicon carbide (SiC) is a typical third-generation semiconductor with wide bandgap and high temperature resistance. High-power devices such as SiC-based field-effect transistors have been successfully developed and have started industrialization in the fields of electric vehicles and power grids. For SiC power devices, the SiC homoepitaxial layer is its core functional area and is the key to ensuring the reliable and stable performance of SiC devices.

[0003] Minority carrier lifetime (minority carrier lifetime) is a key parameter that affects the performance of bipolar devices such as SiC-based insulated gate bipolar transistors (IGBTs). SIC IGBT devices mainly work through minority carrier transport. Improving the minority carrier lifetime in the SiC epitaxial layer can effectively reduce the recombination of minority carriers in the base region, increase the current amplification factor, thereby reducing the on-resistance and improving the performance of SiC IGBT devices. However, in the silicon carbide epitaxial growth process, in order to optimize the defect density in the epitaxial layer, the carbon-silicon ratio used in the growth is usually low, between 0.8-1.2, resulting in a large number of carbon vacancies (point defects) in the epitaxial layer, forming Z 1 / 2 Defects. These point defects become the recombination centers of minority carriers, causing a significant reduction in the minority carrier lifetime. In the current epitaxial process, although the minority carrier lifetime can be optimized to a certain extent by adjusting the growth temperature and other methods, the control range of the minority carrier lifetime is very small. Summary of the invention

[0004] The present application provides a silicon carbide epitaxial growth method and a silicon carbide epitaxial wafer for improving minority carrier lifetime, so as to solve the problem of too short minority carrier lifetime in silicon carbide epitaxial wafer in the prior art.

[0005] In a first aspect, the present application provides a method for epitaxial growth of silicon carbide for improving minority carrier lifetime, comprising: Placing a silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, and sequentially performing etching, buffer layer growth, and drift layer growth on the silicon carbide substrate; After obtaining a drift layer of a first thickness, introducing a carbon source gas into the reaction chamber, and raising the temperature of the reaction chamber to a first preset temperature, carburizing the drift layer to obtain an initial silicon carbide epitaxial wafer; The silicon-containing surface of the initial silicon carbide epitaxial wafer is polished by chemical mechanical polishing technology to obtain a silicon carbide epitaxial wafer containing a drift layer of a target thickness, wherein the first thickness is greater than the target thickness.

[0006] In a possible implementation, after obtaining the drift layer of the first thickness, introducing a carbon source gas into the reaction chamber, raising the temperature of the reaction chamber to a first preset temperature, and carburizing the drift layer to obtain an initial silicon carbide epitaxial wafer, comprising: After obtaining a drift layer of a first thickness, the carbon source gas is introduced into the reaction chamber at a first flow rate, and the temperature of the reaction chamber is increased to a first preset temperature, and the drift layer is carburized for a first period of time to obtain the initial silicon carbide epitaxial wafer.

[0007] In a possible implementation, the flow rate of the first flow rate is in a range of 300-500 sccm.

[0008] In a possible implementation, the first preset temperature ranges from 1700°C to 1900°C.

[0009] In a possible implementation manner, the first time period ranges from 10 to 20 minutes.

[0010] In a possible implementation, placing the silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, and sequentially performing etching, buffer layer growth, and drift layer growth on the silicon carbide substrate includes: Placing the silicon carbide substrate in the reaction chamber, evacuating the reaction chamber, setting the pressure in the evacuated reaction chamber to a predetermined pressure, introducing hydrogen into the reaction chamber at a second flow rate, and raising the temperature in the reaction chamber to a second preset temperature; Introducing hydrogen chloride gas into the reaction chamber at a third flow rate to etch the silicon carbide substrate for a second period of time; After the etching of the silicon carbide substrate is completed, introducing a silicon source gas, a carbon source gas and a dopant of a target concentration into the reaction chamber at a third flow rate to grow a buffer layer on the etched silicon carbide substrate; After the growth of the buffer layer is completed, the silicon source gas, the carbon source gas, and the dopant of the target concentration are introduced into the reaction chamber at a fourth flow rate, and a drift layer of the first thickness is grown on the buffer layer.

[0011] In a possible implementation, the flow rate range of the second flow rate is 50-300 slm; The flow rate of the third flow rate is in the range of 100-500 sccm; The flow rate of the fourth flow rate ranges from 100 to 400 sccm.

[0012] In a possible implementation, the second time period ranges from 5 minutes to 15 minutes; The second preset temperature ranges from 1500°C to 1700°C.

[0013] In a possible implementation manner, a difference between the first thickness and the target thickness is in a range of 1-2 μm.

[0014] In a second aspect, the present application provides a silicon carbide epitaxial wafer, which is prepared using the silicon carbide epitaxial growth method for improving minority carrier lifetime described in the first aspect.

[0015] The present application provides a silicon carbide epitaxial growth method and a silicon carbide epitaxial wafer for improving minority carrier lifetime, by placing a silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, etching the silicon carbide substrate, growing a buffer layer and growing a drift layer in sequence; after obtaining a drift layer of a first thickness, introducing a carbon source gas into the reaction chamber, and raising the temperature of the reaction chamber to a first preset temperature, carburizing the drift layer, and obtaining an initial silicon carbide epitaxial wafer; using chemical mechanical polishing technology, polishing the silicon-containing surface of the initial silicon carbide epitaxial wafer, and obtaining a silicon carbide epitaxial wafer containing a drift layer of a target thickness, wherein the first thickness is greater than the target thickness. The present application effectively reduces the carbon vacancy density in the epitaxial layer and the recombination center of the minority carrier concentration by introducing a carbon source gas for carburizing operation after the drift layer growth is completed, and removes the carbon-rich layer on the surface through surface polishing treatment, and maintains the silicon carbide crystal structure of the epitaxial layer, thereby greatly improving the minority carrier lifetime and surface crystal quality of the silicon carbide epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0017] Figure 1 It is a flow chart of the implementation of the silicon carbide epitaxial growth method for improving minority carrier lifetime provided in the embodiment of the present application; Figure 2 is a schematic structural diagram of an applied silicon carbide epitaxial wafer provided in an embodiment of the present application; Figure 3 It is a schematic diagram of the carburizing operation applied according to the embodiment of the present application. DETAILED DESCRIPTION

[0018] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present application.

[0019] In order to make the purpose, technical solutions and advantages of the present application clearer, specific embodiments will be described below in conjunction with the accompanying drawings.

[0020] Since minority carrier lifetime is a key parameter affecting the performance of bipolar devices such as silicon carbide (SiC)-based insulated gate bipolar transistors (IGBTs), SiC IGBT devices mainly work through minority carrier transport. Improving the minority carrier lifetime in the SiC epitaxial layer can effectively reduce the recombination of minority carriers in the base region, increase the current amplification factor, thereby reducing the on-resistance and improving the performance of SiC IGBT devices. However, in the existing silicon carbide epitaxial growth process, in order to optimize the defect density in the epitaxial layer, the carbon-silicon ratio used in the growth is usually low, between 0.8-1.2, resulting in a large number of carbon vacancies (point defects) in the epitaxial layer, forming Z 1 / 2 Defects. These point defects become the recombination centers of minority carriers, causing a significant reduction in the minority carrier lifetime. In the current epitaxial process, although the minority carrier lifetime can be optimized to a certain extent by adjusting the growth temperature and other methods, the range of minority carrier lifetime regulation is very small.

[0021] In order to solve the problem of short minority carrier lifetime in silicon carbide epitaxial wafers in the prior art mentioned above, the present application reduces the carbon vacancy density in the epitaxial layer and the recombination centers of the minority carrier concentration by adding a surface carburizing process in the epitaxial process, and adds a surface polishing process after the carburizing process to remove the carbon-rich layer on the surface, thereby maintaining the silicon carbide crystal structure of the epitaxial layer, thereby greatly improving the minority carrier lifetime and surface crystallization quality of SiC.

[0022] Figure 1 The implementation flow chart of the silicon carbide epitaxial growth method for improving minority carrier lifetime provided in the embodiment of the present application is described in detail as follows: In step 101, a silicon carbide substrate is placed in a reaction chamber of a silicon carbide epitaxial device, and etching, buffer layer growth and drift layer growth are sequentially performed on the silicon carbide substrate.

[0023] Among them, the growth of silicon carbide epitaxial wafers includes a heating stage, a substrate etching stage, a buffer layer growth stage, a drift layer growth stage and an epitaxial wafer removal stage. In the embodiment of the present application, a carburizing stage is also included after the drift layer growth stage, and a surface polishing stage is also included after the epitaxial wafer removal stage.

[0024] In an embodiment of the present application, a silicon carbide substrate is placed in a reaction chamber of a silicon carbide epitaxial device using a robot, and the silicon carbide substrate is sequentially subjected to a heating stage, a substrate etching stage, a buffer layer growth stage, and a drift layer growth stage to obtain a drift layer of a first thickness.

[0025] At this time, the first thickness of the drift layer is thicker than the target thickness of the drift layer of the device to be finally obtained, so as to reserve a certain thickness margin for subsequent carburizing and polishing operations.

[0026] In a possible implementation, placing a silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, and sequentially performing etching, buffer layer growth, and drift layer growth on the silicon carbide substrate may include: Placing the silicon carbide substrate in a reaction chamber, evacuating the reaction chamber, setting the pressure in the evacuated reaction chamber to a predetermined pressure, introducing hydrogen into the reaction chamber at a second flow rate, and raising the temperature in the reaction chamber to a second preset temperature; Introducing hydrogen chloride gas into the reaction chamber at a third flow rate to etch the silicon carbide substrate for a second period of time; After the etching of the silicon carbide substrate is completed, a silicon source gas, a carbon source gas and a dopant of a target concentration are introduced into the reaction chamber at a third flow rate to grow a buffer layer on the etched silicon carbide substrate; After the growth of the buffer layer is completed, silicon source gas, carbon source gas and dopant of target concentration are introduced into the reaction chamber at a fourth flow rate, and a drift layer of a first thickness is grown on the buffer layer.

[0027] Optionally, a silicon carbide substrate is first placed in a reaction chamber of a silicon carbide epitaxial device using a robot, and the chamber is evacuated, and the pressure in the evacuated reaction chamber is set to a predetermined pressure, and hydrogen is introduced into the reaction chamber at a second flow rate, and the temperature in the reaction chamber is raised to a second preset temperature.

[0028] The purpose of introducing hydrogen into the reaction chamber is to clean the semiconductor surface, remove pollutants and defects such as grease, oxide layer, and occasional metal crystals, so as to ensure the good operation and normal performance of the semiconductor equipment.

[0029] The flow rate of the second flow rate ranges from 50 to 300 slm.

[0030] The second preset temperature, ie, the epitaxial temperature, has a temperature range of 1500°C-1700°C.

[0031] Then, the substrate etching stage is entered, hydrogen chloride gas is introduced into the reaction chamber at a third flow rate, and maintained for a second period of time to perform surface etching of the silicon carbide substrate. Etching the substrate with hydrogen chloride gas can reduce surface damage of the substrate and improve epitaxial quality.

[0032] The flow rate of the third flow rate ranges from 100 to 500 sccm.

[0033] The time period of the second time period ranges from 5 to 15 minutes.

[0034] After the etching of the silicon carbide substrate is completed, the buffer layer growth stage is entered, and silicon source gas, carbon source gas and dopant of target concentration are introduced into the reaction chamber at a third flow rate to grow a buffer layer on the etched silicon carbide substrate.

[0035] The target concentration of the dopant is set according to the required concentration of the silicon carbide epitaxial wafer to be grown.

[0036] In addition, the flow rate range of the third flow rate of the silicon source gas, the carbon source gas, and the dopant of the target concentration is 10-200 sccm.

[0037] The thickness of the buffer layer required to be grown in the embodiment of the present application is in the range of 0.1 μm to 5 μm.

[0038] After the buffer layer grows to the required thickness, the drift layer growth stage is entered, and the silicon source gas, the carbon source gas and the target concentration of the dopant are introduced into the reaction chamber at a fourth flow rate to grow the drift layer to obtain a drift layer of the first thickness. It should be noted that the growth thickness of the drift layer, i.e., the first thickness, should be thicker than the target thickness to facilitate the smooth implementation of the subsequent carburizing and surface polishing processes.

[0039] The target thickness can be customized according to actual needs. The epitaxial thickness is the target thickness, which is determined according to different parameters of product requirements. Depending on the product and the customer, the common target thickness is 6μm, 10μm, etc. In the embodiment of the present application, the first thickness is greater than the target thickness in the range of 1μm-2μm.

[0040] For example, if the customer requires the epitaxial thickness to be 6 μm, the first thickness of the drift layer should be between 7 μm and 8 μm.

[0041] The flow rate range of the fourth flow rate of the silicon source gas, the carbon source gas and the dopant of the target concentration is 100-400 sccm.

[0042] In the embodiment of the present application, after the drift layer growth stage, the drift layer of the first thickness grown reserves additional margin thickness for subsequent carburizing and polishing operations, thereby improving the minority carrier lifetime and surface crystal quality of SiC.

[0043] In step 102, after obtaining a drift layer of a first thickness, a carbon source gas is introduced into the reaction chamber, and the temperature of the reaction chamber is increased to a first preset temperature to carburize the drift layer to obtain an initial silicon carbide epitaxial wafer.

[0044] In an embodiment of the present application, after obtaining a drift layer of the first thickness, the carburizing stage is entered. During the carburizing stage, it is necessary to maintain the second preset temperature, and then the inlet channels of the silicon source gas and the dopant are closed, and only the carbon source gas is introduced into the reaction chamber. After the temperature in the reaction chamber is raised to the first preset temperature, the surface of the drift layer is carburized to obtain an initial silicon carbide epitaxial wafer.

[0045] Since the first preset temperature in the carburizing stage is greater than the second preset temperature in the growth stage, the temperature range of the first preset temperature is 1700°C-1900°C.

[0046] In a possible implementation, after obtaining a drift layer of a first thickness, introducing a carbon source gas into a reaction chamber, and raising the temperature of the reaction chamber to a first preset temperature, carburizing the drift layer to obtain an initial silicon carbide epitaxial wafer may include: After obtaining a drift layer of a first thickness, a carbon source gas is introduced into the reaction chamber at a first flow rate, and the temperature of the reaction chamber is increased to a first preset temperature. The drift layer is carburized for a first period of time to obtain an initial silicon carbide epitaxial wafer.

[0047] Optionally, after obtaining a drift layer of a first thickness, a carburizing stage is entered, wherein the silicon source gas and the dopant are first turned off, and then only the carbon source gas is introduced into the reaction chamber at a first flow rate, and the temperature in the reaction chamber is raised to a first preset temperature, and the surface of the drift layer is carburized for a first time period to obtain an initial silicon carbide epitaxial wafer.

[0048] The flow rate of the first flow rate is in the range of 300-500 sccm.

[0049] The time period for the first time period of continuous carburizing is in the range of 10-20 minutes.

[0050] The embodiment of the present application effectively reduces the carbon vacancy density in the epitaxial layer by introducing a carbon source gas to perform a carburizing operation after the drift layer is grown, thereby reducing the recombination centers of the minority carrier concentration, thereby greatly improving the minority carrier lifetime of SiC.

[0051] In step 103, the silicon-containing surface of the initial silicon carbide epitaxial wafer is polished using chemical mechanical polishing technology to obtain a silicon carbide epitaxial wafer having a drift layer of a target thickness, wherein the first thickness is greater than the target thickness.

[0052] Among them, chemical mechanical polishing (CMP) is a technology that uses a combination of chemical and mechanical methods to precisely grind and polish the surface of silicon wafers.

[0053] In an embodiment of the present application, after obtaining the initial silicon carbide epitaxial wafer, the epitaxial wafer removal stage is first entered, the carbon source gas is turned off, and the reaction chamber is cooled. Subsequently, the initial silicon carbide epitaxial wafer is taken out using a robot, and then the surface polishing stage is entered. The silicon-containing surface of the initial silicon carbide epitaxial wafer is polished using CMP to remove the carbon-rich layer on the surface of the initial silicon carbide epitaxial wafer and at the same time make the thickness of the drift layer reach the target thickness, thereby finally obtaining a silicon carbide epitaxial wafer containing a drift layer of the target thickness.

[0054] The thickness of the drift layer removed by polishing is consistent with the second thickness, which is 1-2 μm.

[0055] The second thickness is a difference between the first thickness and the target thickness.

[0056] In the embodiment of the present application, the carbon-rich layer on the surface of the silicon carbide epitaxial wafer is removed by surface polishing, the silicon carbide crystal structure of the epitaxial layer is maintained, and the surface crystallization quality is improved.

[0057] Exemplarily, the minority carrier lifetimes of silicon carbide epitaxial wafers obtained by using a conventional epitaxial process and a silicon carbide epitaxial growth method for improving minority carrier lifetime provided by the present application are compared in Table 1.

[0058] Table 1 Comparison of minority carrier lifetimes of conventional and improved SiC epitaxial wafers

[0059] It can be clearly seen from Table 1 that the minority carrier lifetime of the silicon carbide epitaxial wafer obtained by the embodiment of the present application is significantly greater than the minority carrier lifetime of the silicon carbide epitaxial wafer under the conventional epitaxial process.

[0060] The present application provides a method for increasing the lifetime of minority carriers in silicon carbide epitaxial growth, by placing a silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, etching the silicon carbide substrate, growing a buffer layer and growing a drift layer in sequence; after obtaining a drift layer of a first thickness, introducing a carbon source gas into the reaction chamber, and raising the temperature of the reaction chamber to a first preset temperature, carburizing the drift layer, and obtaining an initial silicon carbide epitaxial wafer; using chemical mechanical polishing technology, polishing the silicon-containing surface of the initial silicon carbide epitaxial wafer, and obtaining a silicon carbide epitaxial wafer containing a drift layer of a target thickness, wherein the first thickness is greater than the target thickness. The present application effectively reduces the carbon vacancy density in the epitaxial layer and the recombination center of the minority carrier concentration by introducing a carbon source gas for carburizing after the drift layer growth is completed, and removes the carbon-rich layer on the surface through surface polishing, and maintains the silicon carbide crystal structure of the epitaxial layer, thereby greatly increasing the minority carrier lifetime and surface crystal quality of the silicon carbide epitaxial wafer.

[0061] It should be understood that the size of the serial numbers of the steps in the above embodiments does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0062] Figure 2 A physical schematic diagram of a silicon carbide epitaxial wafer provided in an embodiment of the present application is prepared by applying the steps in each of the above-mentioned embodiments of the silicon carbide epitaxial growth method for improving minority carrier lifetime.

[0063] Reference Figure 2 The silicon carbide epitaxial wafer includes a silicon carbide substrate 21, a buffer layer 22 and a drift layer 23. The buffer layer 22 is located above the silicon surface 211 of the silicon carbide substrate 21, and the drift layer 23 is located above the buffer layer 22.

[0064] See also Figure 3 , carbon is infiltrated into the upper surface of the drift layer 23 using a carbon source. The arrow direction is the infiltration direction of carbon.

[0065] The present application provides a silicon carbide epitaxial wafer, which is prepared by the above-mentioned silicon carbide epitaxial growth method for improving minority carrier lifetime. The specific preparation process is: by placing a silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, etching, growing a buffer layer and growing a drift layer on the silicon carbide substrate in sequence; after obtaining a drift layer of a first thickness, introducing a carbon source gas into the reaction chamber, and raising the temperature of the reaction chamber to a first preset temperature, carburizing the drift layer to obtain an initial silicon carbide epitaxial wafer; using chemical mechanical polishing technology, polishing the silicon-containing surface of the initial silicon carbide epitaxial wafer to obtain a silicon carbide epitaxial wafer containing a drift layer of a target thickness, and the first thickness is greater than the target thickness. The present application effectively reduces the carbon vacancy density in the epitaxial layer and reduces the recombination center of the minority carrier concentration by introducing a carbon source gas for carburizing operation after the drift layer growth is completed, and removes the carbon-rich layer on the surface through surface polishing treatment, maintaining the silicon carbide crystal structure of the epitaxial layer, thereby greatly improving the minority carrier lifetime and surface crystal quality of the silicon carbide epitaxial wafer.

[0066] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.

Claims

1. A method for epitaxial growth of silicon carbide to improve minority carrier lifetime, It is characterized in that include: Placing a silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, and sequentially performing etching, buffer layer growth, and drift layer growth on the silicon carbide substrate; After obtaining a drift layer of a first thickness, introducing a carbon source gas into the reaction chamber, and raising the temperature of the reaction chamber to a first preset temperature, carburizing the drift layer to obtain an initial silicon carbide epitaxial wafer; The silicon-containing surface of the initial silicon carbide epitaxial wafer is polished by chemical mechanical polishing technology to obtain a silicon carbide epitaxial wafer containing a drift layer of a target thickness, wherein the first thickness is greater than the target thickness.

2. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 1, It is characterized in that After obtaining the drift layer of the first thickness, introducing a carbon source gas into the reaction chamber, raising the temperature of the reaction chamber to a first preset temperature, and carburizing the drift layer to obtain an initial silicon carbide epitaxial wafer, comprising: After obtaining a drift layer of a first thickness, the carbon source gas is introduced into the reaction chamber at a first flow rate, and the temperature of the reaction chamber is increased to a first preset temperature, and the drift layer is carburized for a first period of time to obtain the initial silicon carbide epitaxial wafer.

3. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 2, It is characterized in that The flow rate of the first flow rate is in the range of 300-500 sccm.

4. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 2, It is characterized in that The temperature range of the first preset temperature is 1700°C-1900°C.

5. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 2, It is characterized in that The first time period ranges from 10 to 20 minutes.

6. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 1, It is characterized in that Placing the silicon carbide substrate in a reaction chamber of a silicon carbide epitaxial device, and sequentially performing etching, buffer layer growth, and drift layer growth on the silicon carbide substrate, comprises: Placing the silicon carbide substrate in the reaction chamber, evacuating the reaction chamber, setting the pressure in the evacuated reaction chamber to a predetermined pressure, introducing hydrogen into the reaction chamber at a second flow rate, and raising the temperature in the reaction chamber to a second preset temperature; Introducing hydrogen chloride gas into the reaction chamber at a third flow rate to etch the silicon carbide substrate for a second period of time; After the etching of the silicon carbide substrate is completed, introducing a silicon source gas, a carbon source gas and a dopant of a target concentration into the reaction chamber at a third flow rate to grow a buffer layer on the etched silicon carbide substrate; After the growth of the buffer layer is completed, the silicon source gas, the carbon source gas, and the dopant of the target concentration are introduced into the reaction chamber at a fourth flow rate, and a drift layer of the first thickness is grown on the buffer layer.

7. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 6, It is characterized in that The flow rate range of the second flow rate is 50-300slm; The flow rate of the third flow rate is in the range of 100-500 sccm; The flow rate of the fourth flow rate ranges from 100 to 400 sccm.

8. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 6, It is characterized in that The time period of the second time period ranges from 5 to 15 minutes; The second preset temperature ranges from 1500°C to 1700°C.

9. The method for epitaxial growth of silicon carbide for improving minority carrier lifetime according to claim 1, It is characterized in that The difference between the first thickness and the target thickness is in the range of 1-2 μm.

10. A silicon carbide epitaxial wafer, It is characterized in that The silicon carbide epitaxial wafer is prepared by using the silicon carbide epitaxial growth method for improving minority carrier lifetime according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for prolonging lifetime of carriers of silicon carbide epitaxial layer

    CN107492482A

  • Substrate and epitaxial wafer

    CN110164959A

  • Method for prolonging service life of silicon carbide epitaxial wafer carrier

    CN114242566A

  • Method for prolonging minority carrier lifetime of silicon carbide epitaxial material

    CN114334609A

  • Silicon carbide epitaxial growth method and equipment

    CN117577514A