IGBT device preparation method and semiconductor device

Repair the height difference on the back of the semiconductor device through laser annealing and etching technology, solving the problem that wet etching cannot remove the abrasive traces, improving electrical properties and reducing the risk of lobes, achieving a more uniform ion distribution and stable collection electrode.

CN118983218APending Publication Date: 2024-11-19成都高投芯未半导体有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411061545.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

After the back process of existing semiconductor devices is thinned, wet etching cannot completely remove the abrasive traces, resulting in a height difference on the back of the wafer, affecting the uniformity of ion distribution and electrical properties, and the bumps generated by the grinding process are difficult to completely remove. Increases lobe risk.

Method used

Laser annealing technology is used to adjust the uniformity of the thinned surface, form a molten layer, and obtain a flatter etching surface through etching, form an anode layer and deposit metal collectors to repair the wafer interface and improve electrical properties.

Benefits of technology

Without increasing equipment costs, the electrical properties of semiconductor devices are improved, the risk of lobes is reduced, and the uniformity of ion distribution and the stability of collectors are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983218A_ABST
    Figure CN118983218A_ABST
Patent Text Reader

Abstract

The invention provides an IGBT (Insulated Gate Bipolar Translator) device preparation method and a semiconductor device, and relates to a semiconductor preparation process. The preparation method of the IGBT device comprises the following steps: providing a wafer; thinning the back surface of the wafer to obtain a thinned surface; and then laser annealing is carried out on the thinned surface to obtain a molten layer so as to adjust the uniformity of the thinned surface. And then etching the fused layer to obtain an etched surface. And finally, forming an anode layer on the etching surface, and depositing metal on the anode layer to form a collector electrode. According to the method, the thinned surface is repaired by using conventional equipment related to back gold processes such as laser annealing to obtain the molten layer, and the molten layer is etched, so that on the basis of not increasing the equipment cost, the height difference of the thinned surface is improved, residual silicon slag on the thinned surface is removed, the purpose of repairing the thinned surface is achieved, and the electrical property of the semiconductor device is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to an IGBT device preparation method and a semiconductor device. Background Art

[0002] Generally, semiconductor devices, such as insulated-gate bipolar transistor (IGBT) chips, will go through backside processing to provide technical support for optimizing the electrical and thermal performance of IGBT chips on the backside, thereby improving the reliability and stability of IGBT chips. Specifically, the backside processing includes backside thinning, ion implantation and other steps in sequence. In addition to reducing the thickness of the chip, backside thinning also needs to provide a smooth metal surface for ion implantation to ensure the uniformity of ion implantation.

[0003] Generally, technicians will use wet etching to remove the grinding gear marks during the back thinning process to repair the rough surface after grinding to a mirror effect, thereby ensuring the uniformity of ion implantation. However, when the back of the wafer after back thinning is directly etched with wet chemicals, even if a mirror effect can be obtained from a macroscopic perspective, in fact, due to the inherent characteristics of wet chemicals, such as the liquid chemicals will flow to the lower part through the grinding gear marks, the back wet etching cannot guarantee the same-side etching; that is, after wet etching, there will still be a height difference of 2 to 3um on the back surface of the wafer, which will affect the uniformity of ion distribution and interfere with the electrical performance of the final semiconductor device. In addition, the grinding process will produce more grinding debris through extrusion, forming bumps on the back of the wafer, and the bumps cannot be completely removed by wet etching, thereby interfering with the electrical properties of the semiconductor device.

[0004] Based on this, there is an urgent need for a semiconductor backside process that can repair the wafer interface and improve the electrical properties of semiconductor devices without increasing equipment costs. Summary of the invention

[0005] The object of the present invention is to provide an IGBT device preparation method and a semiconductor device, which can repair the wafer interface and improve the electrical properties of the semiconductor device without increasing the equipment cost.

[0006] The embodiments of the present invention can be implemented as follows:

[0007] In a first aspect, the present invention provides a method for preparing an IGBT device, comprising the following steps:

[0008] providing a wafer;

[0009] Thinning the back side of the wafer to obtain a thinned surface;

[0010] Performing laser annealing on the thinned surface to obtain a molten layer to adjust the uniformity of the thinned surface;

[0011] Etching the molten layer to obtain an etched surface;

[0012] An anode layer is formed on the etched surface, and metal is deposited on the anode layer to form a collector.

[0013] In one possible implementation, the step of obtaining the molten layer is:

[0014] Using at least two pulsed lasers to sequentially irradiate the thinned surface to change the physical state of the constituent materials of the wafer at the irradiated position, adjust the flatness of the thinned surface, and obtain a molten layer;

[0015] The interval between adjacent pulse lasers is less than the solidification time of the wafer, where the solidification time is used to characterize the time it takes for the constituent material of the wafer at the irradiated position to change from liquid to solid.

[0016] In a possible implementation, the interval time between adjacent pulse lasers satisfies: 0.8us to 1.5us.

[0017] In a possible implementation, the step of sequentially irradiating the thinned surface with at least two pulsed lasers includes:

[0018] For any pulse laser, the pulse laser includes a light spot, and the light spot scans the thinning surface row by row and column by column in sequence; wherein the light spot forms a projection on the thinning surface at each action time, and an overlapping area is formed between adjacent projections.

[0019] In a possible implementation, the total area of ​​the overlapping regions corresponding to the pulsed laser is greater than or equal to 40% of the area of ​​the thinning surface.

[0020] In a possible implementation, when the pulse laser scans row by row and column by column, any vertex of the thinning surface is taken as the origin, and the horizontal and vertical directions are taken as the X-axis direction and the Y-direction respectively;

[0021] The first overlap ratio of the overlapping area in the X-axis direction satisfies: 50% to 90%; wherein the first overlap ratio is used to characterize the overlap ratio of the projections corresponding to adjacent columns in the X-axis direction;

[0022] The second overlap ratio of the overlapping area in the Y-axis direction satisfies: 80% to 90%; wherein the second overlap ratio is used to characterize the overlap ratio of the projections corresponding to adjacent rows in the Y-axis direction.

[0023] In a possible implementation manner, the step of etching the molten layer includes:

[0024] The molten layer on the wafer is etched by wet method to expose the etched surface.

[0025] In a possible implementation manner, the step of forming an anode layer on the etched surface includes:

[0026] Ion implantation and laser annealing are sequentially performed on the etched surface to form an anode layer on the etched surface.

[0027] In a possible implementation, when the thinned surface is subjected to laser annealing, the laser energy satisfies: 3.0 J to 4.5 J, and the laser action time satisfies: 200 ns to 1 ms.

[0028] In a second aspect, the present invention further provides an IGBT device, wherein the semiconductor device is prepared by the IGBT device preparation method described in any one of the first aspects above.

[0029] The beneficial effects of the embodiments of the present invention include, for example:

[0030] Provided are an IGBT device preparation method and a semiconductor device, wherein the IGBT device preparation method comprises: providing a wafer; thinning the back side of the wafer to obtain a thinned surface; then performing laser annealing on the thinned surface to obtain a molten layer to adjust the uniformity of the thinned surface. Subsequently, the molten layer is etched to obtain an etched surface. Finally, an anode layer is formed on the etched surface, and metal is deposited on the anode layer to form a collector. The present invention uses conventional equipment involved in back-gold processes such as laser annealing to repair the thinned surface, obtain a molten layer, and etch the molten layer to improve the height difference of the thinned surface without increasing the equipment cost, remove the silicon slag remaining on the thinned surface, and achieve the purpose of repairing the thinned surface, thereby improving the electrical properties of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 One of the step flow charts of a method for preparing an IGBT device provided by the present invention;

[0033] Figure 2 A second step flow chart of a method for preparing an IGBT device provided by the present invention;

[0034] Figure 3 A schematic diagram of scanning of any laser pulse on the thinning surface in the present invention;

[0035] Figure 4 is the projection image of the spot of any pulsed laser in the present invention in the lower X direction;

[0036] Figure 5 is the projection image of the spot of any pulsed laser in the present invention in the lower Y direction;

[0037] FIG6(A) is a schematic diagram of the flatness of the back side of a wafer under the existing IGBT preparation method;

[0038] FIG. 6(B) is a schematic diagram of the flatness of the back side of the wafer in the IGBT preparation method provided by the present invention. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0040] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in subsequent drawings. At the same time, in the description of this application, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0042] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0043] In the description of the present application, it should be noted that the terms "upper", "lower", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the product of the application is usually placed when in use. They are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0044] In the description of this application, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "disposed" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0045] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0046] As described in the background technology, IGBT chips can provide technical support for the optimization of electrical and thermal performance through the back film forming process. Generally, the back process includes back thinning, ion implantation and other steps in sequence, wherein the back thinning and other related steps are used to provide a smooth metal surface for ion implantation on the basis of reducing the thickness of the IGBT chip, such as the mirror effect described by the technicians, to ensure the uniformity of ion implantation.

[0047] Generally, after the back side of the IGBT chip is thinned, the thinned surface will be etched to remove the grinding wheel marks left during the thinning process. However, researchers have found that the maximum height difference of the grinding wheel marks is about 10um. Direct etching, such as wet etching solution, cannot adjust the thinned surface to a mirror surface from a macroscopic perspective. Because in the actual process, due to the inherent properties of the acid (liquid flows to the lower place), it is impossible to ensure the same-side etching of the thinned surface, that is, there is still a height difference of about 2 to 3um on the thinned surface after etching, and this height difference will directly affect the ion implantation. The impurity ions with the same energy will have different implantation depths with the different heights of the contact surface (during ion implantation, the contact between the ions and the thinned surface after etching, and the thinned surface after etching is defined as the contact surface), resulting in poor uniformity of ion distribution and affecting the electrical properties of the device. In addition, under normal circumstances, the grinding process will cause stress damage to the wafer. Etching alone can only mechanically eliminate the surface effect. If the hidden damage is deep, it cannot be overcome, thereby increasing the risk of cracking in subsequent processes.

[0048] In addition, when the back side of the IGBT chip is thinned, a lot of Si powder (grinding debris) will be crushed onto the back surface of the wafer by the grinding wheel due to the friction of the grinding wheel on the bottom surface of the wafer, forming bumps. The bumps cannot be removed by simple etching, resulting in abnormal contact between the metal film obtained by magnetron sputtering on the thinned surface and the bumps, causing device leakage.

[0049] Based on this, the present invention provides an IGBT device preparation solution, which can repair the wafer interface, improve the electrical properties of the semiconductor device, and reduce the risk of cracking without increasing the equipment cost.

[0050] The embodiments of the present invention can be implemented as follows:

[0051] Please refer to Figure 1 In a first aspect, the present invention provides a method for preparing an IGBT device, comprising steps 110 to 150.

[0052] Step 110: Provide a wafer.

[0053] Step 130 , thinning the back side of the wafer to obtain a thinned surface.

[0054] Step 150 , laser annealing is performed on the thinned surface to obtain a molten layer to adjust the uniformity of the thinned surface.

[0055] Step 160: Etch the molten layer to obtain an etched surface.

[0056] Step 170: forming an anode layer on the etched surface, and depositing metal on the anode layer to form a collector.

[0057] In this embodiment, after the back side of the crystal plane is thinned, laser annealing is performed on the thinned surface to obtain a molten layer through the laser annealing process to improve the thinned surface, and then a more uniform etched surface is obtained through etching, thereby improving the electrical properties of the semiconductor device. In addition, the laser annealing equipment is an existing equipment in the back side process flow of the IGBT device, so the present invention can repair the wafer interface without increasing the equipment cost.

[0058] First, the back side of the wafer is thinned. In one possible implementation, a conventional thinning process and / or a Taiko Grinding thinning process may be used. The Taiko Grinding thinning process may retain a Taiko ring of the original thickness of the wafer on the outside of the wafer; while the conventional thinning process refers to thinning the entire surface without a Taiko ring. In this embodiment, the Taiko Grinding thinning process may be used to thin the back side of the wafer.

[0059] It should be noted that the present application does not limit the wafer thinning thickness or the wafer thickness after thinning, and only needs to meet the requirements of normal wafer manufacturing process. For example, the wafer thinning thickness can meet: 70um ~ 130um.

[0060] In another possible implementation, please refer to Figure 2 Before step 130 of thinning the back side of the wafer to obtain the thinned side, there is a step 120, which is: completing the IGBT front structure on the front side of the wafer, and pasting a protective film on the IGBT front structure to protect the IGBT front structure during the thinning process. In this embodiment, the protective film can be made of UV material.

[0061] In this embodiment, please continue to refer to Figure 2 After completing the thinning process on the back side of the wafer, a step 140 may be further included, and the step 140 is: removing the protective film at the front side structure of the IGBT.

[0062] In this embodiment, after obtaining the corresponding thinned surface and removing the protective film at the front structure of the IGBT, the step 130 of performing laser annealing on the thinned surface to obtain the molten layer is specifically as follows:

[0063] At least two pulsed lasers are used to sequentially irradiate the thinned surface to change the physical state of the wafer constituent material at the irradiated position, adjust the flatness of the thinned surface, and obtain a molten layer.

[0064] Among them, the interval time between adjacent pulse lasers is less than the solidification time of the wafer, and the solidification time is used to characterize the time for the material constituting the wafer at the irradiated position to change from liquid to solid.

[0065] This embodiment uses a pulsed laser to irradiate the thinned surface, so as to adjust the flatness of the thinned surface by laser annealing to obtain a molten layer. In this way, the present invention can adjust the temperature or action time of laser annealing to make the wafer surface, especially the thinned surface, so that the silicon on the thinned surface quickly melts to form a liquid state, and completes the replacement of the lattice structure during the high-temperature residence or melting process, that is, recrystallization, repairs the silicon lattice, and reduces the risk of cracking. At the same time, high temperature or a longer action time can directly melt the silicon residue remaining on the wafer surface during the thinning process, avoid leakage of IGBT devices, and ensure the electrical properties of semiconductor devices.

[0066] In one possible implementation, based on the thickness of the IGBT device after thinning, and in order to avoid wafer fragments caused by excessive energy, when each laser pulse in the present invention performs laser annealing on the thinned surface, the laser energy satisfies: 3.0J~4.5J, and the laser action time satisfies: 200ns~1ms.

[0067] During the laser annealing process, at least two pulsed lasers may be used to scan the thinned surface in sequence to increase the action time of the corresponding thinned surface and make the back side of the wafer more uniform. In a possible implementation, the interval time between adjacent pulsed lasers satisfies: 0.8us to 1.5us.

[0068] In this embodiment, the positions of the laser pulses acting on the thinning surface are the same. Figure 3 , Figure 3 The figure shows a schematic diagram of the scanning of the laser pulse on the thinning surface; assuming that each laser pulse starts scanning from the upper left corner of the thinning surface, the laser transmitter can send the first laser pulse and the second laser pulse in sequence at a unit time interval of 1.2us, that is, the emission time of the second laser pulse is later than the first laser pulse, and the time difference is 1.2us. At this time, the projection positions of each laser pulse on the thinning surface are the same, so that the thermal budget of the back surface of the wafer is sufficient, and the temperature is sufficient to melt the silicon.

[0069] It should be noted that the interval between adjacent pulse lasers is less than the solidification time of the wafer, and the solidification time is used to characterize the time for the composition of the wafer at the irradiation position to change from liquid to solid. Specifically, after the first laser pulse is emitted (irradiated on the thinning surface), the silicon at the corresponding irradiation position can be melted by the preset laser energy and the preset laser action time. For example, the laser energy is 4.5J, and the laser action time is 500ns. After a corresponding 1.2us time interval, the second laser pulse is irradiated at the same action position, and the wafer is processed with a laser energy of 4.5J and a laser action time of 500ns. At this time, the 1.2us time interval can ensure that when the second laser pulse starts to act, the silicon at the corresponding action position is still in a melted or semi-solidified state, so that the thermal budget of the back surface of the wafer is sufficient by using multiple laser pulses, and the silicon at the scanning position is ensured to be in a melted state, thereby greatly eliminating the height difference of the thinning surface.

[0070] In this embodiment, the steps of sequentially irradiating the thinning surface with at least two pulsed lasers are specifically as follows:

[0071] For any pulse laser, the pulse laser includes a light spot, and the light spot scans the thinning surface row by row and column by column in sequence; wherein the light spot forms a projection on the thinning surface at each action time, and an overlapping area is formed between projections located adjacently.

[0072] Please continue to refer to Figure 3 , Figure 3The projection image of the light spot under any pulse laser is also shown; the pulse laser is provided by the laser annealing machine, and when the pulse laser is projected on the thinning surface, a light spot is formed. During laser annealing, the wafer carrier will move the wafer in a preset direction so that the light spot acts on multiple preset positions on the wafer. In this embodiment, each pulse laser forms a light spot, and the light spot of each pulse laser scans row by row and column by column on the thinning surface.

[0073] In order to maximize the thermal budget of the back surface of the wafer, the silicon at the scanning position is kept in a molten state, thereby minimizing the height difference of the thinning surface. Figure 4 , Figure 4 The projection image of the spot of any pulsed laser in the present embodiment in the lower X direction is shown; wherein, with the upper left corner of the thinning surface as the origin, and the horizontal and vertical directions as the X-axis direction and the Y-direction respectively, multiple projections corresponding to at least 4 rows and 4 columns are displayed on the thinning surface. Taking the multiple projections corresponding to the number of rows N=2 as an example, the first row of projections is represented by the projection corresponding to the number of rows N=2 and the number of columns M=1; the second row of projections is represented by the projection corresponding to the number of rows N=2 and the number of columns M=2; the third row of projections is represented by the projection corresponding to the number of rows N=2 and the number of columns M=3; the fourth row of projections is represented by the projection corresponding to the number of rows N=2 and the number of columns M=4.

[0074] Please continue to refer to Figure 4 , assuming that the spot corresponding to any laser pulse forms 4 projections on the X-axis direction (each row) of the thinning surface, wherein each projection is formed by a spot under a pulse laser at different action times. For example, the first row of projections is formed by the spot under the pulse laser at 0 ns, the second row of projections is formed by the spot under the pulse laser at 500 ns, the third row of projections is formed by the spot under the pulse laser at 1000 ns, and the fourth row of projections is formed by the spot under the pulse laser at 1500 ns. It can be understood that each time the spot of the pulse laser forms a spot at the action time of 500 ns, it will move along the X-axis direction to form corresponding multiple rows of projections.

[0075] An overlapping area is formed between the second row of projections and the third row of projections in the X-axis direction. It is understandable that when the pulse laser scans line by line, an overlapping area is formed between projections located adjacently. In a possible implementation, the first overlapping rate of the overlapping area in the X-axis direction may satisfy: 50% to 90%. The first overlapping rate is used to characterize the overlapping ratio of projections corresponding to adjacent columns in the X-axis direction.

[0076] Specifically, taking the overlapping area formed between the second row projection and the third row projection as an example, the first overlapping ratio represents the overlapping ratio between adjacent column projections corresponding to the same row in the X-axis direction, and the overlapping ratio is the ratio of the length of the overlapping area to the length between projections.

[0077] It should be noted that, for the convenience of description, Figure 4 Only the overlapping area formed between the second and third rows of projections in the X-axis direction is shown, and corresponding overlapping areas are formed between the other adjacent rows of projections. That is, the overlapping areas between the first and second rows of projections, and between the third and fourth rows of projections in the X-axis direction are similar to the overlapping areas between the second and third rows of projections.

[0078] Similarly, see Figure 5 , Figure 5 The projection image of the spot of a pulsed laser in the lower Y direction in this embodiment is shown; wherein, with the upper left corner of the thinning surface as the origin, and the horizontal and vertical directions as the X-axis direction and the Y-direction respectively, multiple projections corresponding to at least 4 rows and 4 columns are displayed on the thinning surface. Taking the multiple projections corresponding to the number of columns M=2 as an example, the first column of projections represents the projection corresponding to the number of rows N=1 and the number of columns M=2; the second column of projections represents the projection corresponding to the number of rows N=2 and the number of columns M=2; the third column of projections represents the projection corresponding to the number of rows N=3 and the number of columns M=2; and the fourth column of projections represents the projection corresponding to the number of rows N=4 and the number of columns M=2.

[0079] Please continue to refer to Figure 5 , assuming that the light spot corresponding to any laser pulse forms 4 projections in the Y-axis direction (each row) of the thinning surface, wherein each projection is formed by a light spot under a pulse laser at different action times. Among them, an overlapping area is formed between the second column projection and the third column projection in the Y-axis direction. It can be understood that when the pulse laser scans row by row, an overlapping area is formed between the adjacent column projections. In one possible implementation method, the second overlap rate of the overlapping area in the Y-axis direction can meet: 80% to 90%; wherein the second overlap rate is used to characterize the overlap ratio of the projections corresponding to adjacent rows in the Y-axis direction.

[0080] Specifically, taking the overlapping area formed between the second column projection and the third row column projection as an example, the second overlapping rate represents the overlapping ratio between adjacent column projections in the same column in the Y-axis direction, which is the ratio between the width of the overlapping area and the width between projections.

[0081] In this embodiment, the total area of ​​the overlapping regions corresponding to the pulsed laser is greater than or equal to 40% of the area of ​​the thinning surface.

[0082] In one possible implementation, the step of etching the molten layer includes:

[0083] The molten layer on the wafer is wet etched to expose the etched surface.

[0084] In this embodiment, after the molten layer formed in the laser annealing is wet-etched, the height difference of the surface where the molten layer is located is small enough, so the wet etching solution can etch downward more evenly to expose a more uniform back surface of the wafer. At this time, the back surface of the wafer will not affect the subsequent process of preparing the anode layer.

[0085] In one possible implementation, the step of forming an anode layer on the etched surface includes:

[0086] Ion implantation and laser annealing are performed sequentially on the etched surface to form an anode layer on the etched surface.

[0087] In this embodiment, ion implantation can be performed on the etched surface, for example, phosphorus ion implantation and boron ion implantation into the etched surface, and then a second laser annealing is performed to activate the implanted ions to form an anode layer. Then, metal Al / Ti / Ni / Ag is deposited on the back of the wafer to form a back collector.

[0088] It should be noted that, in this embodiment, the anode layer can be understood as a field stop layer and a collector region formed by ion implantation on the etched surface.

[0089] It should be noted that the second laser annealing does not limit the injection energy, delay time and corresponding overlap rate, wherein the injection energy and other settings can be matched with the type of ion implanted particles (P+ or B+) and the injection depth. During the second laser annealing, if the energy is too high, it will affect the final distribution depth of the ion laser. However, the energy used in this process often cannot achieve the purpose of removing silicon residues.

[0090] Please refer to Figure 6(A) and Figure 6(B), wherein Figure 6(A) and Figure 6(B) show a comparison of the flatness of the back side of the wafer under the existing IGBT preparation method and the IGBT preparation method of the present invention; wherein Figure 6(A) is a schematic diagram of the flatness of the back side of the wafer under the existing IGBT preparation method; and Figure 6(B) is a schematic diagram of the flatness of the back side of the wafer under the IGBT preparation method provided by the present invention. It can be clearly seen that the IGBT preparation method provided by the present invention can significantly improve the flatness of the back side of the wafer.

[0091] In summary, the present invention provides a method for preparing an IGBT device, wherein the method for preparing an IGBT device comprises: providing a wafer; thinning the back side of the wafer to obtain a thinned surface; and then performing laser annealing on the thinned surface to obtain a molten layer to adjust the uniformity of the thinned surface. The molten layer is then etched to obtain an etched surface. Finally, an anode layer is formed on the etched surface, and metal is deposited on the anode layer to form a collector. The present invention uses conventional equipment that may be involved in back-gold processes such as laser annealing to repair the thinned surface, obtain a molten layer, and etch the molten layer to improve the height difference of the thinned surface without increasing the equipment cost, remove the silicon slag remaining on the thinned surface, and achieve the purpose of repairing the thinned surface, thereby improving the electrical properties of the semiconductor device.

[0092] In a second aspect, the present invention further provides an IGBT device, wherein the semiconductor device is prepared by any IGBT device preparation method of the first aspect.

[0093] Among them, the IGBT device provided by the present invention uses conventional equipment involved in back-gold processes such as laser annealing to repair the thinned surface, obtain a molten layer, and etch the molten layer to improve the height difference of the thinned surface without increasing the equipment cost, remove the silicon slag remaining on the thinned surface, and achieve the purpose of repairing the thinned surface, thereby improving the electrical properties of the semiconductor device.

[0094] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

[0095] It will be apparent to those skilled in the art that the present application is not limited to the details of the exemplary embodiments described above, and that the present application can be implemented in other specific forms without departing from the spirit or essential features of the present application. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the present application is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present application. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing an IGBT device, characterized in that: The following steps are involved: providing a wafer; Thinning the back side of the wafer to obtain a thinned surface; Performing laser annealing on the thinned surface to obtain a molten layer to adjust the uniformity of the thinned surface; Etching the molten layer to obtain an etched surface; An anode layer is formed on the etched surface, and metal is deposited on the anode layer to form a collector.

2. The method for preparing an IGBT device according to claim 1, characterized in that: The steps of obtaining the molten layer are: Using at least two pulsed lasers to sequentially irradiate the thinned surface to change the physical state of the constituent materials of the wafer at the irradiated position, adjust the flatness of the thinned surface, and obtain a molten layer; The interval between adjacent pulse lasers is less than the solidification time of the wafer, where the solidification time is used to characterize the time it takes for the constituent material of the wafer at the irradiated position to change from liquid to solid.

3. The method for preparing an IGBT device according to claim 2, characterized in that: The interval time between adjacent pulse lasers satisfies: 0.8us to 1.5us.

4. The method for preparing an IGBT device according to claim 2, characterized in that: The step of sequentially irradiating the thinning surface with at least two pulsed lasers comprises: For any pulse laser, the pulse laser includes a light spot, and the light spot scans the thinning surface row by row and column by column in sequence; wherein the light spot forms a projection on the thinning surface at each action time, and an overlapping area is formed between adjacent projections.

5. The method for preparing an IGBT device according to claim 4, characterized in that: The total area of ​​the overlapping regions corresponding to the pulse laser is greater than or equal to 40% of the area of ​​the thinning surface.

6. The method for preparing an IGBT device according to claim 4, characterized in that: When the pulse laser scans row by row and column by column, any vertex of the thinning surface is taken as the origin, and the horizontal and vertical directions are taken as the X-axis direction and the Y-direction respectively; The first overlap ratio of the overlapping area in the X-axis direction satisfies: 50% to 90%; wherein the first overlap ratio is used to characterize the overlap ratio of the projections corresponding to adjacent columns in the X-axis direction; The second overlap ratio of the overlapping area in the Y-axis direction satisfies: 80% to 90%; wherein the second overlap ratio is used to characterize the overlap ratio of the projections corresponding to adjacent rows in the Y-axis direction.

7. The method for preparing an IGBT device according to claim 1, characterized in that: The step of etching the molten layer comprises: The molten layer on the wafer is etched by wet method to expose the etched surface.

8. The method for preparing an IGBT device according to claim 1, characterized in that: The step of forming an anode layer on the etched surface comprises: Ion implantation and laser annealing are sequentially performed on the etched surface to form an anode layer on the etched surface.

9. The method for preparing an IGBT device according to claim 1 or 2, characterized in that: When the thinned surface is subjected to laser annealing, the laser energy satisfies: 3.0 J to 4.5 J, and the laser action time satisfies: 200 ns to 1 ms.

10. An IGBT device, characterized in that: The semiconductor device is manufactured by the IGBT device manufacturing method according to any one of claims 1 to 9.