Thermal switch regulation and control type polymer modified positive electrode material as well as preparation method and application thereof

By using PMMA-PAN and 2-methylpropane coating on the positive electrode material of lithium-ion battery and combining silicone rubber penetration technology, a thermal switch-regulated polymer-modified positive electrode material is formed, which solves the thermal stability and safety of lithium-ion batteries. The effect of preventing the spread of battery heat at high temperatures is achieved.

CN118983402AActive Publication Date: 2024-11-19VKAN CERTIFICATION & TESTING +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410922381.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-19
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

While the existing lithium-ion battery positive electrode materials increase the energy density, the thermal stability decreases, which easily leads to thermal runaway and battery explosion. The existing polymer coating technology mainly improves electrical conductivity and ignores the inhibition of thermal spread.

Method used

The positive electrode active particles are coated with PMMA-PAN and 2-methylpropane, and the mechanical stability is improved through silicone rubber penetration, forming a thermal switch-regulated polymer-modified positive electrode material, which can switch the thermal conductivity state to the insulating state at high temperatures to prevent The battery heat spreads.

Benefits of technology

Improve the electrical performance and thermal safety of the battery under normal working conditions, ensure the uniform distribution of the battery temperature, and quickly reduce the thermal conductivity at high temperatures, prevent the battery from spreading heat and avoid explosions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983402A_ABST
    Figure CN118983402A_ABST
Patent Text Reader

Abstract

The invention discloses a thermal switch regulation and control type polymer modified positive electrode material which is characterized by comprising positive electrode active particles, silicone rubber and a polymer layer, and the polymer layer comprises a polymethyl methacrylate-polyacrylonitrile copolymer and 2-methyl propane. The positive electrode material has a thermal switch regulation and control function, can ensure that the battery has excellent electrical properties under a normal working condition, can switch a heat conduction state of the battery into a heat insulation state under a high-temperature condition, and effectively prevents heat spreading of the battery. The invention also discloses a preparation method of the positive electrode material and an application of the positive electrode material in a battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a thermal switch controllable polymer modified positive electrode material and a preparation method and application thereof. Background Art

[0002] Driven by energy transformation and dual carbon goals, the application of lithium-ion batteries in electric vehicles, large-scale power grids and storage, and low-altitude economy has shown large-scale growth. As market demand continues to rise, the research and development of low-cost, high-energy-density and high-safety lithium-ion batteries is also imminent. At present, the main way to obtain high-energy-density lithium-ion batteries is to increase the capacity of positive electrode materials; however, increasing the capacity of positive electrode materials usually causes the thermal stability of the battery to decrease, which can easily cause thermal runaway and lead to heat spread in the battery, and even fire and explosion.

[0003] The common technical route at present is to match a high-nickel, pressure-resistant positive electrode with a silicon-carbon negative electrode to increase the battery energy density and meet the endurance requirements. However, the thermal stability of the high-nickel ternary material used in the above positive electrode is relatively poor. When the temperature inside the battery rises, the positive electrode material is prone to lattice distortion or collapse, aggravating the temperature rise, leading to thermal runaway, and inevitably catastrophic battery explosion. When the high-energy-density battery is at 100-200°C, the silicon-carbon negative electrode first undergoes thermal runaway, and the heat diffuses to the positive electrode, causing the positive electrode material to decompose, releasing oxygen to react with the electrolyte, and further increasing the battery temperature, forming a positive feedback loop of thermal energy, and eventually catching fire and exploding. This type of battery fire and explosion accident seriously endangers the personal and property safety of consumers. Therefore, it is necessary to propose an effective solution to suppress thermal runaway or heat spread of positive electrode materials in terms of lithium-ion safety.

[0004] In addition, the use of polymers to coat positive electrode materials is one of the common ways to modify positive electrode materials. Most modifications aim to improve the conductivity of the composite material, thereby improving the overall electrical performance of the battery.

[0005] For example, prior art 1: China's published patent CN114335467 A discloses a coated modified layered LiMO2 positive electrode material and a preparation method thereof, wherein the LiMO2 positive electrode material is coated with a cyclized layer PAN, and at the same time, the surface layered phase is induced to transform into a rock salt phase, thereby obtaining a layered phase-rock salt phase-PAN surface coupling structure, thereby improving the electrochemical activity of the positive electrode material.

[0006] Another example is prior art 2: China's patent CN107507961 B discloses a method for preparing a conductive polymer modified positive electrode sheet for a lithium-ion battery, wherein polyvinyl carbazole is coated on the surface of a positive electrode active material of a lithium-ion battery, and then the positive electrode active material coated with polyvinyl carbazole is coated on a current collector to prepare a positive electrode sheet for a lithium-ion battery. This patent can effectively reduce the interfacial side reactions between the positive electrode active material and the electrolyte, and can also ensure that lithium ions have a good transfer efficiency, while also enhancing the conductivity of the positive electrode material and extending the service life of the positive electrode active material.

[0007] The purpose of the above-mentioned prior art to use polymer to coat the positive electrode material is to improve the conductivity of the positive electrode material, but there is a lack of research on the thermal stability of the positive electrode material. While modifying the positive electrode material of the battery to improve the battery capacity and cycle life, the prior art ignores key safety issues, especially the limited ability to inhibit the spread of battery heat, which hinders the further development of the technology. Summary of the invention

[0008] One of the purposes of the present invention is to provide a thermal switch control type polymer modified positive electrode material, which has a thermal switch control function, can ensure that the battery has excellent electrical properties under normal working conditions, can switch the battery's thermal conductive state to an insulating state under high temperature conditions, and effectively prevent heat spread in the battery.

[0009] The second object of the present invention is to provide a method for preparing the above-mentioned thermal switch controllable polymer modified positive electrode material.

[0010] The third object of the present invention is to provide an application of the above-mentioned thermal switch controllable polymer modified positive electrode material.

[0011] The first invention objective of the present invention is achieved through the following technical solutions.

[0012] A thermal switch control type polymer modified positive electrode material, characterized in that it comprises positive electrode active particles, silicone rubber and a polymer layer;

[0013] The polymer layer includes polymethyl methacrylate-polyacrylonitrile copolymer (hereinafter referred to as: PMMA-PAN) and 2-methylpropane.

[0014] The polymer layer is coated on the surface of the positive electrode active particles. The silicone rubber is used to penetrate the positive electrode active particles coated with PMMA-PAN and 2-methylpropane.

[0015] The present invention is the first to use PMMA-PAN and 2-methylpropane to coat the positive electrode active particles, and combines silicone rubber infiltration to improve the mechanical stability of the positive electrode material, so that the modified positive electrode material has a thermal switch control function. The application of this modified positive electrode material in the battery can, on the one hand, improve the thermal conductivity of the battery to ensure that it obtains excellent electrical performance under normal working conditions, and on the other hand, it can quickly convert the battery from a thermal conductive state at room temperature to an insulating state at high temperature, thereby inhibiting the thermal spread of the battery; specifically, when the battery is at room temperature, the thermal switch control type polymer modified positive electrode material provides a good heat transfer loop, ensuring that the battery temperature is evenly distributed under normal working conditions, and is conducive to accelerating lithium ion migration and increasing battery capacity; when the battery is at a high temperature, the lattice structure of the positive electrode active particles is distorted or collapsed, and the polymer layer expands in volume, destroying the heat transfer loop, resulting in a rapid decrease in the thermal conductivity of the thermal switch control type polymer modified positive electrode material, thereby preventing the battery from thermal spread.

[0016] The coating amount of the polymer layer is 0.08-2wt% of the mass of the positive electrode active particles. When the coating amount of the polymer layer is 0.08-2wt%, the positive electrode active particles can be uniformly coated and the thickness of the polymer layer can be avoided to be too large, thereby providing the polymer modified positive electrode material with better thermal conductivity. When the coating amount of the polymer layer is less than 0.8wt%, the thickness of the polymer layer is thin, and the coating uniformity is poor. The coating layer is dotted or intermittently coated, and the heat transfer channel of the positive electrode material is uneven. When the temperature rises, due to the poor coating effect of the polymer layer, the thermal conductivity is maintained at a high level, and it is impossible to quickly achieve insulation, and even the heat spreads outward; when the polymer coating layer is greater than 2wt%, the polymer layer is significantly thickened, and the heat transfer channel is too long, which hinders the conduction of solid-phase lithium ions and affects the capacity of the positive electrode material under normal working conditions. Preferably, the coating amount of the polymer layer is 1wt% of the mass of the positive electrode active particles.

[0017] The thickness of the polymer layer is 3-10 nm, preferably 5 nm.

[0018] In the polymer-modified positive electrode material, the mass of the silicone rubber is 1-2 wt % of the mass of the positive electrode active particles.

[0019] The silicone rubber is polydimethylsiloxane rubber.

[0020] The positive electrode active particles can be selected from the layered structure Li x M y O2 (M = Co, Ni, Mn), spinel structure LiMn2O4, olivine structure LiFePO4, and transition metal oxides Na x MeO2 (Me=Mn, Fe, Ni, Co, V, Cu, Cr, etc.), polyanionic compounds Nax M y (X a O b ) z Z w (M=Fe, V, Ni, Co, etc., X=P, Si, S, etc. and Z=F-, OH-, etc.), Bruce blue compounds Na x MA[MB(CN)6]·nH2O (MA and MB are transition metal ions), etc.

[0021] The polymer modified positive electrode material also includes an organic binder, which is one or more of polyvinylidene fluoride (PVDF), polyvinyl pyrrolidone, and sucrose; the amount of the organic binder is 1 to 100 wt % of the mass of the positive electrode active particles.

[0022] The second invention objective of the present invention is achieved through the following technical solutions.

[0023] The method for preparing the thermal switch controllable polymer modified positive electrode material is characterized by comprising the following steps:

[0024] (1) mixing an organic binder and a solvent to obtain an organic solvent slurry; adding a polymer to the organic solvent slurry, stirring the mixture to obtain a positive electrode material slurry, and further stirring the mixture to obtain a positive electrode material slurry, and placing the mixture in a drying oven for heating and degassing; the polymer includes PMMA-PAN and 2-methylpropane;

[0025] (2) pouring the positive electrode material slurry obtained in step (1) into a mold and cooling it in liquid nitrogen; taking the frozen sample out of the mold and drying it with a freeze dryer to obtain polymer-coated positive electrode active particles;

[0026] (3) uniformly mixing the silicone rubber base material and the curing agent to obtain a silicone rubber precursor; then infiltrating the silicone rubber precursor into the polymer-coated positive electrode active particles, and curing them in a drying oven to obtain the thermal switch controllable polymer modified positive electrode material.

[0027] The organic binder is one or more of polyvinylidene fluoride (PVDF), polyvinyl pyrrolidone, and sucrose; the amount of the organic binder is 1 to 100 wt % of the mass of the positive electrode active particles.

[0028] The solvent is one or more of N-methylpyrrolidone (NMP) and propylene oxide (ECH), and the volume dosage thereof is 1-2 mL: 1 g to the mass of the positive electrode active particles.

[0029] The added amount of PMMA-PAN and 2-methylpropane is 0.8-2wt% of the mass of the positive electrode active particles to ensure that the polymer layer is evenly coated and has an appropriate thickness.

[0030] In step (1), the polymer further comprises one or more of polyacrylonitrile, poly (3,4-ethylenedioxythiophene) / polystyrene sulfonate (PEDOT:PSS), and the amount of the polymer added is 0.8 to 100 wt % of the mass of the positive electrode active particles.

[0031] In step (1), the temperature in the drying oven is 60 to 90°C.

[0032] In step (2), the positive electrode material slurry is poured into the mold and then cooled for 1 to 10 minutes, and then dried in a freeze dryer for 24 to 60 hours.

[0033] In step (3), the silicone base material is polydimethylsiloxane, the curing agent is a silane coupling agent, and the mass ratio of the silicone base material to the curing agent is 5:1 to 20:1.

[0034] In step (3), the infiltration amount of the silicone rubber precursor is 1 to 2 wt % of the mass of the positive electrode active particles, and the infiltration time is 6 to 8 hours.

[0035] In step (3), the curing temperature in the drying oven is 60 to 90°C.

[0036] The third invention objective of the present invention is achieved through the following technical solutions.

[0037] The above-mentioned thermal switch controllable polymer modified positive electrode material is used in batteries to improve the thermal safety performance of the batteries.

[0038] The battery comprises a positive electrode sheet, a separator and a negative electrode sheet stacked in sequence, the positive electrode sheet comprises a current collector and a positive electrode active slurry coated on the current collector, and the positive electrode active slurry comprises the thermal switch control type polymer modified positive electrode material.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The present invention coats a polymer layer on the surface of the positive electrode active particles and infiltrates silicone rubber thereon to obtain the thermal switch control type polymer modified positive electrode material; the present invention utilizes the structure of polymer layer coating and silicone rubber infiltration to enable the positive electrode material to obtain a thermal switch control function; the positive electrode material not only improves the electrical performance of the battery, but also improves the thermal safety of the battery, switches the thermal conductive state of the battery to the thermal insulation state under high temperature conditions, and inhibits heat spread in the battery.

[0041] When the battery is at room temperature, the thermal switch-regulated polymer-modified positive electrode material has a good heat transfer circuit, and the thermal conductivity is increased, ensuring that the battery temperature is evenly distributed under normal working conditions, and can accelerate the migration of lithium ions, increase the mobility, thereby increasing the battery capacity, and increasing the battery energy density;

[0042] When the battery is at high temperature, the lattice structure of the positive electrode active particles is distorted or collapsed, and the polymer layer expands in volume, destroying the heat transfer circuit, causing the thermal conductivity of the thermal switch-regulated polymer-modified positive electrode material to drop rapidly, putting the battery in an insulating state, preventing heat from spreading in the battery, and avoiding catastrophic battery explosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 is a graph showing the change in thermal conductivity of the battery of Example 4 as the temperature applied thereto by the variable temperature test system increases;

[0044] Figure 2 It is a curve diagram showing the change of battery temperature over time in Examples 4, 5 and 6 and Comparative Examples 7 and 8 during the temperature application process of the variable temperature test system. DETAILED DESCRIPTION

[0045] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] The present invention uses LiNi 0.8 Co 0.1 Mn 0.1 O2 (with an average particle size of 2-10 μm and an average specific surface area of ​​0.45 m 2 / g) as positive electrode active particles for specific implementation, the technical solution of the present invention is specifically described. The raw materials used in the following examples are all commercially available products; PMMA-PAN and 2-methylpropane are Matsumoto Microsphere HF-48D products purchased from Matsumoto Yushi-Seiyaku Company, which consists of PMMA-PAN as the shell and 2-methylpropane as the core.

[0047] Example 1

[0048] The thermal switch controllable polymer modified positive electrode material of this embodiment includes positive electrode active particles, silicone rubber and a polymer layer coated on the positive electrode active particles. The coating amount of the polymer layer is 0.8wt% and the thickness of the polymer layer is 3nm.

[0049] The specific implementation is as follows:

[0050] Step 1: Weigh 5 g of PVDF and 150 mL of NMP into a beaker and stir. Mix well to obtain an organic solvent slurry; add 0.8 g of PMMA-PAN and 2-methylpropane to the organic solvent slurry and stir. After stirring well, add 100 g of positive electrode active particles and stir further to obtain positive electrode material slurry, which is placed in an 85°C drying oven for heating and degassing.

[0051] Step 2: Place the PTFE (polytetrafluoroethylene) mold on a copper plate wrapped with aluminum foil, pour the positive electrode material slurry obtained in step 1 into the mold, and cool it in liquid nitrogen for 5 minutes. Take the frozen sample out of the mold and dry it in a freeze dryer for 48 hours to obtain polymer-coated positive electrode active particles.

[0052] Step 3: Mix polydimethylsiloxane and silane coupling agent in a mass ratio of 15:1 to obtain a polydimethylsiloxane rubber precursor; then add the precursor to the polymer-coated positive electrode active particles and infiltrate them for 8 hours, the infiltration amount accounting for 1wt% of the mass of the positive electrode active particles, and cure them in a drying oven at 85°C to form a thermal switch-regulated polymer-modified positive electrode material.

[0053] The thickness of the polymer layer in the thermal switch controllable polymer modified positive electrode material obtained in this embodiment is 3 nm, and the polymer layer is evenly coated.

[0054] Example 2

[0055] The thermal switch controllable polymer modified positive electrode material of this embodiment includes positive electrode active particles, silicone rubber and a polymer layer coated on the positive electrode active particles. The coating amount of the polymer layer is 1wt% and the thickness of the polymer layer is 5nm.

[0056] The specific implementation is as follows:

[0057] Step 1: Weigh 5g PVDF and 150mL NMP into a beaker and stir. Mix well to obtain an organic solvent slurry; add 1g PMMA-PAN and 2-methylpropane to the organic solvent slurry and stir. After stirring well, add 100g positive electrode active particles and stir further to obtain positive electrode material slurry, which is placed in an 85°C drying oven for heating and degassing.

[0058] Step 2: Place the PTFE (polytetrafluoroethylene) mold on a copper plate wrapped with aluminum foil, pour the positive electrode material slurry obtained in step 1 into the mold, and cool it in liquid nitrogen for 5 minutes. Take the frozen sample out of the mold and dry it in a freeze dryer for 48 hours to obtain polymer-coated positive electrode active particles.

[0059] Step 3: Mix polydimethylsiloxane and silane coupling agent in a mass ratio of 15:1 to obtain a polydimethylsiloxane rubber precursor; then add the precursor to the polymer-coated positive electrode active particles and infiltrate them for 6 hours, the infiltration amount accounting for 1wt% of the mass of the positive electrode active particles, and cure them in a drying oven at 85°C to form a thermal switch-regulated polymer-modified positive electrode material.

[0060] The thickness of the polymer layer in the thermal switch controllable polymer modified positive electrode material obtained in this embodiment is 5 nm, and the polymer layer is evenly coated.

[0061] Example 3

[0062] The thermal switch controllable polymer modified positive electrode material of this embodiment includes positive electrode active particles, silicone rubber and a polymer layer coated on the positive electrode active particles. The coating amount of the polymer layer is 1.5wt% and the thickness of the polymer layer is 8nm.

[0063] The specific implementation is as follows:

[0064] Step 1: Weigh 5 g of PVDF and 150 mL of NMP into a beaker and stir to obtain an organic solvent slurry; add 1.5 g of PMMA-PAN and 2-methylpropane to the organic solvent slurry and stir to obtain a positive electrode material slurry, which is then placed in an 85°C drying oven for heating and degassing.

[0065] Step 2: Place the PTFE (polytetrafluoroethylene) mold on a copper plate wrapped with aluminum foil, pour the positive electrode material slurry obtained in step 1 into the mold, and cool it in liquid nitrogen for 5 minutes. Take the frozen sample out of the mold and dry it in a freeze dryer for 48 hours to obtain polymer-coated positive electrode active particles.

[0066] Step 3: Mix polydimethylsiloxane and silane coupling agent in a mass ratio of 15:1 to obtain a polydimethylsiloxane rubber precursor; then add the precursor to the polymer-coated positive electrode active particles and infiltrate them for 6 hours, the infiltration amount accounting for 1wt% of the mass of the positive electrode active particles, and cure them in a drying oven at 85°C to form a thermal switch-regulated polymer-modified positive electrode material.

[0067] The thickness of the polymer layer in the thermal switch controllable polymer modified positive electrode material obtained in this embodiment is 8 nm, and the polymer layer is evenly coated.

[0068] Comparative Example 1

[0069] The thermal switch control type polymer modified positive electrode material of this comparative example includes positive electrode active particles, silicone rubber and a polymer layer coated on the positive electrode active particles, the coating amount of the polymer layer is 0.04wt%, and the thickness of the polymer layer is 1nm.

[0070] The specific implementation is as follows:

[0071] Step 1: Weigh 5g PVDF and 150mL NMP into a beaker and stir to prepare an organic solvent slurry; add 0.04g PMMA-PAN and 2-methylpropane to the organic solvent slurry and stir, then add 100g positive electrode active particles and stir further to obtain positive electrode material slurry, which is placed in an 85°C drying oven for heating and degassing.

[0072] Step 2: Place the PTFE (polytetrafluoroethylene) mold on a copper plate wrapped with aluminum foil, pour the positive electrode material slurry obtained in step 1 into the mold, and cool it in liquid nitrogen for 5 minutes. Take the frozen sample out of the mold and dry it with a freeze dryer for 48 hours to obtain polymer-coated positive electrode active particles.

[0073] Step 3: Mix polydimethylsiloxane and silane coupling agent in a mass ratio of 15:1 to obtain a polydimethylsiloxane rubber precursor; then add the precursor to the polymer-coated positive electrode active particles and infiltrate them for 6 hours, the infiltration amount accounting for 1wt% of the mass of the positive electrode active particles, and cure them in a drying oven at 85°C to obtain a polymer-modified positive electrode material.

[0074] The thickness of the polymer layer in the positive electrode material obtained in this comparative example is 1 nm, and the coating is discontinuous, which indicates that the coating amount of the polymer layer used in this comparative example is too low.

[0075] Comparative Example 2

[0076] The thermal switch controllable polymer modified positive electrode material of this comparative example comprises positive electrode active particles, silicone rubber and a polymer layer coated on the positive electrode active particles, wherein the coating amount of the polymer layer is 4wt% and the thickness of the polymer layer is 15nm.

[0077] The specific implementation is as follows:

[0078] Step 1: Weigh 5g PVDF and 150mL NMP into a beaker and stir. After mixing evenly, an organic solvent slurry is prepared; 4g PMMA-PAN and 2-methylpropane are added to the organic solvent slurry and stirred. After stirring evenly, 100g positive electrode active particles are added and further stirred to obtain a positive electrode material slurry, which is placed in an 85°C drying oven for heating and degassing.

[0079] Step 2: Place the PTFE (polytetrafluoroethylene) mold on a copper plate wrapped with aluminum foil, pour the positive electrode material slurry obtained in step 1 into the mold, and cool it in liquid nitrogen for 5 minutes. Take the frozen sample out of the mold and dry it in a freeze dryer for 48 hours to obtain polymer-coated positive electrode active particles.

[0080] Step 3: Mix polydimethylsiloxane and silane coupling agent in a mass ratio of 15:1 to obtain a polydimethylsiloxane rubber precursor; then add the precursor to the polymer-coated positive electrode active particles and infiltrate them for 6 hours, the infiltration amount accounting for 1wt% of the mass of the positive electrode active particles, and cure them in a drying oven at 85°C to form a polymer-modified positive electrode material.

[0081] The thickness of the polymer layer in the positive electrode material obtained in this comparative example is 10 nm, and it is a thick coating.

[0082] Comparative Example 3

[0083] The difference between this comparative example and Example 2 is that PMMA-PAN and 2-methylpropane are not added in step 1. The remaining steps are the same as those in Example 2.

[0084] Comparative Example 4

[0085] This comparative example is a positive electrode active material without any coating, that is, positive electrode active particles.

[0086] Thermal conductivity tests were performed on the positive electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4. The results are shown in Tables 1 to 3.

[0087] Table 1

[0088] Example <![CDATA[Thermal conductivity (Wm -1 K -1 )]]> Temperature(℃) Example 1 1.03 25 Example 2 1.33 25 Example 3 1.15 25

[0089] The polymer layers of Examples 1 to 3 uniformly coat the positive electrode active particles. As shown in Table 1, at 25°C, the thermal switch regulated polymer modified positive electrode material of the present invention has good thermal conductivity, and when the polymer layer coating amount is 1wt%, it exhibits the best thermal conductivity of 1.33Wm -1 K -1 .

[0090] Table 2

[0091] Example <![CDATA[Thermal conductivity (Wm -1 K -1 )]]> Temperature(℃) Example 2 1.33 25 Comparative Example 1 0.61 25 Comparative Example 2 0.56 25

[0092] It can be seen from the data in Table 2 that at 25°C, too high or too low a coating amount of the polymer layer will affect the thermal conductivity of the positive electrode material.

[0093] Table 3

[0094]

[0095]

[0096] From the data in Table 3, it can be seen that at 25°C, the thermal conductivity of the positive electrode active particles of Comparative Example 4 is 0.45 Wm -1 K -1 , while the thermal conductivity of the positive electrode material of Comparative Example 3, which is not coated with PMMA-PAN and 2-methylpropane, is only 0.52 Wm -1 K -1 However, the thermal conductivity (1.33 Wm -1 K -1 ). This indicates that in the thermal switch controllable polymer modified positive electrode material of the present invention, the polymer layer can provide a good heat transfer channel at room temperature, thereby improving lithium ion migration and improving the performance of the positive electrode sheet.

[0097] Example 4

[0098] (1) preparing a battery: coating a positive electrode active slurry with the thermal switch controllable polymer modified positive electrode material of Example 2 as the main component on a current collector to obtain a positive electrode sheet; then sequentially stacking the positive electrode sheet, the separator and the negative electrode sheet to obtain a battery;

[0099] (2) The battery obtained in step (1) was placed in a charge and discharge test system, charged and discharged at a rate of 1C, with a charge cut-off voltage of 4.3V and a discharge cut-off voltage of 2.7V. The initial capacity of the battery was tested, and the battery capacity was tested again after 100 cycles. The results are shown in Table 4;

[0100] (3) The battery obtained in step (1) was placed in a variable temperature test system, and the temperature was set to rise from 25°C to 300°C at a heating rate of 5°C / min. The thermal conductivity of the battery and its temperature change were tested. The results were as follows: Figure 1 and 2 shown.

[0101] Example 5

[0102] (1) preparing a battery: coating a positive electrode active slurry containing the thermal switch controllable polymer modified positive electrode material of Example 1 as a main component on a current collector to obtain a positive electrode sheet; then sequentially stacking the positive electrode sheet, the separator and the negative electrode sheet to obtain a battery;

[0103] (2) The battery obtained in step (1) was placed in a charge and discharge test system, charged and discharged at a rate of 1C, with a charge cut-off voltage of 4.3V and a discharge cut-off voltage of 2.7V. The initial capacity of the battery was tested, and the battery capacity was tested again after 100 cycles. The results are shown in Table 4;

[0104] (3) The battery obtained in step (1) was placed in a variable temperature test system, and the temperature was set to rise from 25°C to 300°C at a heating rate of 5°C / min. The temperature change of the battery was tested. The results were as follows: Figure 2 shown.

[0105] Example 6

[0106] (1) preparing a battery: coating a positive electrode active slurry with the thermal switch controllable polymer modified positive electrode material of Example 3 as the main component on a current collector to obtain a positive electrode sheet; then sequentially stacking the positive electrode sheet, the separator and the negative electrode sheet to obtain a battery;

[0107] (2) The battery obtained in step (1) was placed in a charge and discharge test system, charged and discharged at a rate of 1C, with a charge cut-off voltage of 4.3V and a discharge cut-off voltage of 2.7V. The initial capacity of the battery was tested, and the battery capacity was tested again after 100 cycles. The results are shown in Table 4;

[0108] (3) The battery obtained in step (1) was placed in a variable temperature test system, and the temperature was set to rise from 25°C to 300°C at a heating rate of 5°C / min. The temperature change of the battery was tested. The results were as follows: Figure 2 shown.

[0109] Comparative Example 5

[0110] The difference between this comparative example and Example 4 is that the positive electrode active slurry with the positive electrode material of Comparative Example 1 as the main component is coated on the current collector. The remaining experimental steps are consistent with Example 4.

[0111] Comparative Example 6

[0112] The difference between this embodiment and embodiment 4 is that the positive electrode active slurry with the positive electrode material of comparative example 2 as the main component is coated on the current collector. The remaining experimental steps are consistent with those of embodiment 4.

[0113] Comparative Example 7

[0114] The difference between this embodiment and embodiment 4 is that the positive electrode active slurry with the positive electrode material of comparative example 3 as the main component is coated on the current collector. The remaining experimental steps are consistent with those of embodiment 4.

[0115] Comparative Example 8

[0116] The difference between this embodiment and embodiment 4 is that the positive electrode active slurry with the positive electrode material of comparative example 4 as the main component is coated on the current collector. The remaining experimental steps are consistent with those of embodiment 4.

[0117] Table 4

[0118]

[0119] It can be seen from the data in Table 4 that the battery in Comparative Example 7, which uses positive electrode active materials that have not been coated with PMMA-PAN and 2-methylpropane, exhibits low thermal conductivity, low gram capacity, and poor cycle stability; the battery in Comparative Example 8, which uses positive electrode active particles that have not undergone any coating modification, exhibits even worse thermal conductivity, lower gram capacity, and even worse cycle stability. Examples 4, 5, and 6 of the present invention all exhibit relatively high thermal conductivity and gram capacity, especially Example 4 exhibits excellent thermal conductivity and capacity, which indicates that the application of the thermal switch-regulated polymer-modified positive electrode material of the present invention to batteries can improve the electrical performance of the battery at room temperature. However, the batteries in Comparative Examples 5 and 6 exhibit inferior thermal conductivity and gram capacity to those in Examples 4 to 6 because the polymer layer of the positive electrode material is not uniformly coated or the thickness is too high.

[0120] Depend on Figure 1 The data show that the battery of Example 4 adopts the thermal switch control type polymer modified positive electrode material of the present invention, and its thermal conductivity gradually decreases with the increase of the applied temperature, especially when it is greater than 100°C, the thermal conductivity decreases to 0.4 Wm -1 K -1 This indicates that the polymer-modified positive electrode material of the present invention has a thermal switch regulation function, which can ensure the thermal conductivity of the material under normal working conditions, and switch to an adiabatic state when the temperature is higher than 100°C. This is mainly due to the unique structural design of the present invention. When the battery is at high temperature, the lattice structure of the positive electrode active particles is distorted or collapsed, and the polymer layer expands in volume, which destroys the heat transfer circuit and causes a rapid decrease in thermal conductivity.

[0121] Figure 2 The figure is a graph showing the relationship between the battery temperature of Example 4, Example 5, Example 6 and Comparative Example 7 and Comparative Example 8 and the time during the temperature application process of the variable temperature test system. Figure 2 The data shows that when thermal runaway occurs, the battery using polymer-modified positive electrode materials controls the temperature rise of the battery within less than 350 seconds; while for batteries using positive electrode active materials that have not been coated with PMMA-PAN and 2-methylpropane, and batteries using positive electrode active particles that have not been modified in any way, the temperature of both continues to rise over time, which may cause the battery to catch fire. This shows that the application of the thermal switch-regulated polymer-modified positive electrode material of the present invention to batteries can effectively prevent the spread of the battery and improve the thermal safety of the battery.

Claims

1. A thermal switch control type polymer modified positive electrode material, characterized in that: It includes positive electrode active particles, silicone rubber and a polymer layer; The polymer layer includes polymethyl methacrylate-polyacrylonitrile copolymer and 2-methylpropane.

2. The thermal switch controllable polymer modified positive electrode material according to claim 1, characterized in that: The coating amount of the polymer layer is 0.08-2wt% of the mass of the positive electrode active particles; the mass of the silicone rubber is 1-2wt% of the mass of the positive electrode active particles.

3. The thermal switch controllable polymer modified positive electrode material according to claim 2, characterized in that: The thickness of the polymer layer is 3-10 nm.

4. The thermal switch controllable polymer modified positive electrode material according to claim 3, characterized in that: The silicone rubber is polydimethylsiloxane rubber; the positive electrode active particles are selected from the layered structure Li of the Li system x M y One of O2, spinel structure LiMn2O4, and olivine structure LiFePO4.

5. The method for preparing the thermal switch controllable polymer modified positive electrode material according to claim 1, characterized in that: The following steps are involved: (1) mixing an organic binder and a solvent to obtain an organic solvent slurry; adding a polymer to the organic solvent slurry, stirring the mixture to obtain a positive electrode material slurry, and further stirring the mixture to obtain a positive electrode material slurry, and placing the mixture in a drying oven for heating and degassing; the polymer comprises a polymethyl methacrylate-polyacrylonitrile copolymer and 2-methylpropane; (2) pouring the positive electrode material slurry obtained in step (1) into a mold and cooling it in liquid nitrogen; taking the frozen sample out of the mold and drying it with a freeze dryer to obtain polymer-coated positive electrode active particles; (3) uniformly mixing the silicone rubber base material and the curing agent to obtain a silicone rubber precursor; then infiltrating the silicone rubber precursor into the polymer-coated positive electrode active particles, and curing them in a drying oven to obtain the thermal switch controllable polymer modified positive electrode material.

6. The method for preparing the thermal switch controllable polymer modified positive electrode material according to claim 5, characterized in that: The organic binder is one or more of polyvinylidene fluoride, polyvinyl pyrrolidone and sucrose; the amount of the organic binder is 1 to 100 wt% of the mass of the positive electrode active particles; The solvent is one or more of N-methylpyrrolidone and propylene oxide, and the volume amount thereof is 1-2 mL: 1 g to the mass of the positive electrode active particles; The amount of PMMA-PAN and 2-methylpropane added is 0.8-2 wt % of the mass of the positive electrode active particles.

7. The method for preparing the thermal switch controllable polymer modified positive electrode material according to claim 6, characterized in that: In step (3), the silicone base material is polydimethylsiloxane, the curing agent is a silane coupling agent, and the mass ratio of the silicone base material to the curing agent is 5:1 to 20:1; the impregnation amount of the silicone rubber precursor is 1 to 2 wt% of the mass of the positive electrode active particles, and the impregnation time is 6 to 8 hours.

8. The method for preparing the thermal switch controllable polymer modified positive electrode material according to claim 7, characterized in that: In step (1), the polymer further comprises one or more of polyacrylonitrile, poly (3,4-ethylenedioxythiophene) / polystyrene sulfonate.

9. The method for preparing the thermal switch controllable polymer modified positive electrode material according to claim 8, characterized in that: In step (1) and step (3), the temperature in the drying oven is 60 to 90° C.; in step (2), the positive electrode material slurry is poured into the mold and then cooled for 1 to 10 minutes and dried in a freeze dryer for 24 to 60 hours.

10. Use of the thermal switch controllable polymer modified positive electrode material according to claim 1 in a battery.

Citation Information

Patent Citations

  • A method for preparing a conductive polymer-modified positive electrode sheet for lithium-ion batteries

    CN107507961B

  • Coated modified layered LiMO2 positive electrode material and preparation method thereof

    CN114335467A

  • Method for improving safety of lithium ion battery

    CN112332030A

  • Preparation method of lithium ion battery positive electrode material with thermal shutdown and self-healing functions

    CN112382746A

  • Positive plate and lithium ion battery comprising same

    CN115642221A