Preparation method and application of hollow spherical CoNi2S4-coated C nano composite material

The preparation of hollow spherical CoNi2S4@C nanocomposite material by solvent thermal method solves the problems of cumbersome preparation steps and poor reproducibility of CoNi2S4 materials in the prior art, and achieves efficient and stable sodium ion electrochemical storage and excellent battery performance.

CN118983412AActive Publication Date: 2024-11-19HEFEI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411059281.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-03
Publication Date
2024-11-19
Estimated Expiration
2044-08-03

AI Technical Summary

Technical Problem

The prior art has cumbersome steps, complex processes and poor reproducibility when preparing CoNi2S4 nanocomposites, resulting in poor electrical conductivity and poor cycle stability, which makes it impossible to meet the needs of sodium ion battery negative electrode materials.

Method used

Using the solvothermal synthesis method, hollow spherical CoNi2S4@C nanometers were prepared by adding cobalt, nickel, sulfur, cetyl trimethylammonium bromide and glucose to the ethylene glycol solution. Composite material, simplifying the process and improving the specific surface area and porosity of the material.

Benefits of technology

It realizes efficient and stable sodium ion electrochemical storage, improves the structural stability and sodium storage performance of the material, and significantly improves the reversible capacity, rate performance and cycling performance of the negative electrode material of sodium ion battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983412A_ABST
    Figure CN118983412A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a hollow spherical CoNi2S4-coated C nano composite material, and belongs to the technical field of sodium ion battery negative electrode materials. The preparation method comprises the following steps: dissolving a cobalt source, a nickel source and a sulfur source in an ethylene glycol solution, adding cetyltrimethylammonium bromide (CTAB) and glucose, uniformly stirring, putting the obtained solution in a high-temperature and high-pressure reaction kettle, and reacting to obtain the CoNi2S4atC nano composite material. The preparation method is simple and high in repeatability, the diameter size of the prepared CoNi2S4 at C hollow nanosphere is 400-600 nm, and the CoNi2S4 at C hollow nanosphere has the advantages of being large in specific surface area and good in conductivity. When the material is used as a sodium ion battery negative electrode material, a carbon coating structure on the surface and an internal hollow structure of the material can effectively relieve volume change in the charge-discharge process, so that the material shows relatively high reversible capacity and excellent rate capability and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of negative electrode materials for sodium ion batteries, and specifically relates to a preparation method and application of a hollow spherical CoNi2S4@C nanocomposite material. Background Art

[0002] In recent years, with the widespread application of lithium-ion batteries in the fields of energy storage and power vehicles, their limitations have gradually emerged, such as the cost problem caused by limited lithium resources, the problem of capacity attenuation in low temperature environments, and safety issues during use. These unfavorable factors have affected the further development of lithium-ion batteries. Sodium and lithium are in the same main group and have many similar physical and chemical properties. In addition, sodium resources are abundant, widely distributed, and low in cost. When sodium-ion batteries are rapidly charged and discharged, it is not easy for sodium to precipitate at the negative electrode. They are highly safe and have good low-temperature performance. Therefore, sodium-ion batteries are considered to be the next generation of electrochemical energy storage technology with great application potential.

[0003] As a new type of negative electrode material for sodium ion batteries, CoNi2S4 has the advantages of relatively abundant resources, high theoretical capacity, good conductivity, stable thermal and mechanical properties, and Na + It has the advantages of good diffusion kinetics and environmental friendliness, and is a sodium-ion battery negative electrode material with great application prospects.

[0004] At present, the methods for preparing transition metal sulfides including CoNi2S4 mostly use the solid phase method (CVD method). This method is not only cumbersome, complex and has poor reproducibility, but also the prepared CoNi2S4 particles are large and the morphology is mostly uncontrollable, resulting in the material's conductivity still not being ideal. It cannot adapt to large volume changes during repeated sodium insertion and extraction, resulting in electrode pulverization and poor cycle stability.

[0005] Therefore, it is of great research value and significance to find a simple, highly reproducible and morphology-controllable method to prepare CoNi2S4 nanocomposites to achieve efficient, stable and safe electrochemical storage of sodium ions. Summary of the invention

[0006] In view of the fact that carbon coating and morphology control are effective strategies for modifying electrode materials, the present invention aims at the shortcomings of current CoNi2S4 negative electrode materials and provides a method for preparing a hollow spherical CoNi2S4@C nanocomposite material with simple preparation process, high repeatability and excellent electrochemical performance.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A preparation method of a hollow spherical CoNi2S4@C nanocomposite material is synthesized by a solvothermal method. First, a cobalt source, a nickel source and a sulfur source are dissolved in an ethylene glycol solution. Then, cetyltrimethylammonium bromide (CTAB) and glucose are added and mixed and stirred evenly. Then, the reaction solution is placed in a reaction container for solvothermal reaction. After the reaction is completed, the hollow spherical CoNi2S4@C nanocomposite material is obtained through post-treatment.

[0009] As a preferred technical solution of the present invention, the cobalt source, nickel source and sulfur source are added in an atomic ratio of 1:2:6, and the molar concentration of cobalt atoms in the reaction system is 0.01-0.05 mol / L.

[0010] As a preferred technical solution of the present invention, the cobalt source is cobalt acetate, cobalt nitrate or cobalt chloride; the nickel source is nickel acetate, nickel nitrate or nickel chloride; and the sulfur source is sodium thiosulfate or sodium sulfide.

[0011] As a preferred technical solution of the present invention, the molar concentration of hexadecyltrimethylammonium bromide in the reaction system is 0.05-0.20 mol / L, and the molar concentration of glucose in the reaction system is 0.01-0.05 mol / L.

[0012] As a preferred technical solution of the present invention, the cetyltrimethylammonium bromide (CTAB) and glucose are added and stirred for 0.5 to 2 hours at a stirring speed of 400 to 500 r / min.

[0013] As a preferred technical solution of the present invention, the solvent thermal reaction temperature is 160-200° C., and the reaction time is 18-24 hours.

[0014] As a preferred technical solution of the present invention, the post-treatment is to remove the upper solution by high-speed centrifugation after the reaction is completed to obtain a black precipitate, and then use ethanol and deionized water to centrifuge and wash several times respectively, and then vacuum dry to obtain a hollow spherical CoNi2S4@C nanomaterial.

[0015] The present invention prepares a hollow spherical CoNi2S4@C nanocomposite material from a cobalt source, a nickel source, and a sulfur source by a one-step solvothermal method. The hollow spherical CoNi2S4@C nanocomposite material has a high specific surface area and porosity, can effectively increase its contact area with the electrolyte, and has a large number of chemical reaction active sites on its surface and inside. When used as a negative electrode material for a sodium ion battery, the battery has a higher specific capacity. In addition, due to the introduction of the carbon coating structure, the hollow spherical structure of the product is stable and has a good rigid structure, which can effectively alleviate the problem of volume expansion of the electrode material during the charge and discharge process. Therefore, the hollow spherical CoNi2S4@C nanomaterial prepared by the present invention can effectively improve the structural stability and sodium storage performance of the negative electrode material of the sodium ion battery.

[0016] Compared with the prior art, the beneficial effects of the present invention are also shown in:

[0017] (1) The present invention uses a one-step solvent thermal method for preparation, which is simple and fast, with a short experimental cycle, low cost and high repeatability.

[0018] (2) The CoNi2S4@C material prepared by the method of the present invention is in the shape of nano hollow spheres with a diameter of 400-600nm. It has the characteristics of large specific surface area and good conductivity. Its large specific surface area increases the contact area between the electrode material and the electrolyte, providing more active sites for electrochemical reactions; its large porosity is conducive to the rapid diffusion of sodium ion batteries; its surface carbon coating structure and internal hollow structure can effectively alleviate the volume change during the charge and discharge process, thus showing a high reversible capacity, as well as excellent rate performance and cycle performance.

[0019] (3) The hollow spherical CoNi2S4@C nanocomposite material prepared by the present invention has a high reversible capacity, as well as excellent rate and cycle performance when used as a negative electrode material for sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XRD pattern of the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention.

[0021] Figure 2 This is a scanning electron microscope photograph of the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention.

[0022] Figure 3 Transmission electron microscopy and mapping photos of the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention.

[0023] Figure 4 This is the Raman spectrum of the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention.

[0024] Figure 5 This is the rate performance curve of a sodium ion battery assembled using the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention as the battery negative electrode material.

[0025] Figure 6 This is the cycle performance curve of a sodium ion battery assembled using the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention as the battery negative electrode material at 10C.

[0026] Figure 7 This is the electrochemical impedance curve of the hollow spherical CoNi2S4@C nanocomposite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The following is a clear introduction to the preparation scheme of the hollow spherical CoNi2S4@C nanocomposite material in the embodiment of the present invention in conjunction with the accompanying drawings in the embodiment. The described embodiments are only some embodiments of the present invention, not all embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. The structure and morphological properties of the product obtained by the method of the present invention are characterized and analyzed by field emission scanning electron microscopy (FE-SEM, SU8010) and X-ray powder diffraction (XRD, Smart Lab) and other instruments.

[0028] Example 1

[0029] The preparation method of hollow spherical CoNi2S4@C nanocomposite material comprises the following specific steps:

[0030] Step 1: Weigh 0.1245 g of cobalt acetate (tetrahydrate), 0.249 g of nickel acetate (tetrahydrate), and 0.747 g of sodium thiosulfate (pentahydrate) and add them to 30 mL of ethylene glycol.

[0031] Step 2: Add 1 g of hexadecyltrimethylammonium bromide and 0.1 g of glucose to the solution obtained in step 1, and mix and stir for 1 hour at a rotation speed of 500 r / min.

[0032] Step 3: Transfer the solution obtained in step 2 to a stainless steel reactor lined with polytetrafluoroethylene, and keep it at 180°C for 20 hours using a forced air drying oven.

[0033] Step 4: After the reaction is completed, the upper liquid is removed by centrifugation to obtain a black precipitate, which is centrifugally washed multiple times with ethanol and deionized water. The obtained sample is placed in a vacuum drying oven and vacuum dried at 80°C for 12 hours.

[0034] Please also read Figures 1 to 4 7. The sample prepared in Example 1 was analyzed by X-ray diffractometer and found to have the same structure as CoNi2S4 (JCPDS: 24-0334), indicating that CoNi2S4@C was successfully prepared using the method in this example. The sample was observed by field emission scanning electron microscopy and transmission electron microscopy, and it can be seen that the prepared CoNi2S4@C nanocomposite material is a spherical structure with a diameter of 400-600nm, a hollow interior, a rough surface, and a uniform coating of carbon material. The Raman spectrum of the sample shows that the I D (disordered or defective carbon) / I G The ratio of (graphite carbon) is 1.11, indicating that the sample has more defective structures and good electrical conductivity.

[0035] The hollow spherical CoNi2S4@C nanocomposite prepared in this example was made into a slurry and coated on the surface of copper foil, and then assembled with a sodium sheet into a half-cell, and its electrochemical performance was tested. The electrochemical test results are shown in Figure 2. Figure 5 , 6 As shown: At a current density of 10A / g, the first discharge specific capacity is as high as 689.98mAh / g. After 1000 charge and discharge cycles, its capacity retention rate is as high as 71.84%, showing a high reversible capacity, as well as good rate and cycle performance.

[0036] Example 2

[0037] The preparation method of hollow spherical CoNi2S4@C nanocomposite material comprises the following specific steps:

[0038] Step 1: Weigh 0.249 g of cobalt acetate (tetrahydrate), 0.498 g of nickel acetate (tetrahydrate), and 1.494 g of sodium thiosulfate (pentahydrate) and add them to 30 mL of ethylene glycol.

[0039] Step 2: Add 2 g of hexadecyltrimethylammonium bromide and 0.2 g of glucose to the solution obtained in step 1, and mix and stir for 2 h at a rotation speed of 500 r / min.

[0040] Step 3: Transfer the solution obtained in step 2 to a stainless steel reactor lined with polytetrafluoroethylene, and keep it at 200° C. for 24 h in a forced air drying oven.

[0041] Step 4: After the reaction is completed, the upper liquid is removed by centrifugation to obtain a black precipitate, which is centrifugally washed multiple times with ethanol and deionized water. The obtained sample is placed in a vacuum drying oven and vacuum dried at 80°C for 12 hours.

[0042] The hollow spherical CoNi2S4@C nanocomposite prepared in this example was made into a slurry and coated on the surface of copper foil, and then assembled with a sodium sheet into a half-cell, and its electrochemical performance was tested. The electrochemical test results showed that at a current density of 10A / g, the initial discharge capacity was 663.02mAh / g, and after 1000 charge and discharge cycles, its capacity retention rate was 70.92%.

[0043] Example 3

[0044] The preparation method of hollow spherical CoNi2S4@C nanocomposite material comprises the following specific steps:

[0045] Step 1: Weigh 0.1245 g of cobalt acetate (tetrahydrate), 0.249 g of nickel acetate (tetrahydrate), and 0.747 g of sodium thiosulfate (pentahydrate) and add them to 30 mL of ethylene glycol.

[0046] Step 2: Add 0.75 g of hexadecyltrimethylammonium bromide and 0.08 g of glucose to the solution obtained in step 1, and mix and stir for 0.5 h at a rotation speed of 400 r / min.

[0047] Step 3: Transfer the solution obtained in step 2 to a stainless steel reactor lined with polytetrafluoroethylene, and keep it at 160° C. for 18 h in a forced air drying oven.

[0048] Step 4: After the reaction is completed, the upper liquid is removed by centrifugation to obtain a black precipitate, which is centrifugally washed multiple times with ethanol and deionized water. The obtained sample is placed in a vacuum drying oven and vacuum dried at 80°C for 12 hours.

[0049] The hollow spherical CoNi2S4@C nanocomposite prepared in this example was made into a slurry and coated on the surface of copper foil, and then assembled with a sodium sheet into a half-cell, and its electrochemical performance was tested. The electrochemical test results showed that at a current density of 10A / g, the initial discharge capacity was 647.24mAh / g, and after 1000 charge and discharge cycles, its capacity retention rate was 70.21%.

[0050] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a hollow spherical CoNi2S4@C nanocomposite material, synthesized by a solvothermal method, characterized in that: First, the cobalt source, nickel source and sulfur source are dissolved in ethylene glycol solution, and then cetyltrimethylammonium bromide (CTAB) and glucose are added and mixed and stirred evenly. Then, the reaction solution is placed in a reaction container for solvothermal reaction. After the reaction is completed, hollow spherical CoNi2S4@C nanocomposite materials can be obtained through post-treatment.

2. The preparation method according to claim 1, characterized in that The cobalt source, nickel source and sulfur source are added in an atomic ratio of 1:2:6, and the molar concentration of cobalt atoms in the reaction system is 0.01-0.05 mol / L.

3. The preparation method according to claim 2, characterized in that: The cobalt source is cobalt acetate, cobalt nitrate or cobalt chloride; the nickel source is nickel acetate, nickel nitrate or nickel chloride; and the sulfur source is sodium thiosulfate or sodium sulfide.

4. The preparation method according to claim 2, characterized in that: The molar concentration of the hexadecyltrimethylammonium bromide in the reaction system is 0.05-0.20 mol / L, and the molar concentration of glucose in the reaction system is 0.01-0.05 mol / L.

5. The preparation method according to claim 1, characterized in that: After the cetyltrimethylammonium bromide (CTAB) and glucose are added, they are stirred and mixed for 0.5 to 2 hours at a stirring speed of 400 to 500 r / min.

6. The preparation method according to claim 1, characterized in that: The solvent thermal reaction temperature is 160-200° C., and the reaction time is 18-24 hours.

7. The preparation method according to claim 1, characterized in that: The post-treatment is to remove the upper solution by high-speed centrifugation after the reaction is completed, thereby obtaining a black precipitate, and wash it by centrifugation for several times with ethanol and deionized water respectively, and then obtain a hollow spherical CoNi2S4@C nanomaterial by vacuum drying.

8. The CoNi2S4@C nanomaterial prepared by the method according to any one of claims 1 to 7, characterized in that The microstructure is nano-spherical with a hollow interior and a sphere diameter of 400 to 600 nm.

9. Use of the hollow spherical CoNi2S4@C nanocomposite material obtained by the preparation method according to any one of claims 1 to 7 or according to claim 8 as a negative electrode material for sodium ion batteries.

Citation Information

Patent Citations

  • Method for synthesizing Fe3O4 / C lithium ion battery cathode material with hollow sphere structure by one-step process

    CN102208641A

  • Carbon-coated nickel sulfide electrode material and preparation method and application thereof

    CN112018344A

  • Hollow spherical bimetallic chalcogenide, preparation method and sodium battery negative electrode

    CN112803017A

  • Method for preparing dielectric carbon coated hollow Co9S8 microspheres of sodium ion battery negative electrode material

    CN114464801A

  • Yolk shell structure CoNi2S4 / GDY composite material as well as preparation method and application thereof

    CN117275957A