Method for repairing and regenerating waste lithium iron phosphate positive electrode material
By combining anaerobic roasting and UV irradiation pretreatment with heat treatment, the problems of complex recycling processes and high energy consumption of lithium iron phosphate batteries have been solved, enabling efficient regeneration and industrial application of waste lithium iron phosphate cathode materials.
Patent Information
- Application Number
- CN202411058241.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium iron phosphate battery recycling processes are complex and energy-intensive, and traditional recycling processes are not suitable for industrial applications.
A pretreatment method involving anaerobic calcination and ultraviolet irradiation, combined with the reaction of lithium source and dopamine in Tris-hydrochloric acid buffer, followed by heat treatment for lithium intercalation and surface carbonization, was used to achieve the repair and regeneration of lithium iron phosphate materials.
The process has been simplified, energy consumption has been reduced, and efficient regeneration of waste lithium iron phosphate cathode materials has been achieved, making it suitable for industrial application.
Smart Images

Figure CN118983438A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recovery and regeneration, and relates to a method for repairing and regenerating waste lithium iron phosphate positive electrode materials. Background Art
[0002] Lithium iron phosphate batteries have become the leader among various lithium-ion battery cathode materials due to their low cost, high safety and durability, and are widely used in electric vehicles and smart grids. With the rapid growth of the number of electric vehicles worldwide, millions of tons of lithium iron phosphate batteries that are about to reach the end of their service life need to be properly disposed of. The hydrometallurgical recycling of waste lithium iron phosphate batteries is a complicated process that consumes a large amount of chemicals and produces a large amount of wastewater that needs to be treated. The pyrometallurgical calcination process consumes a lot of energy and has very limited lithium recovery. Considering the low-cost manufacturing of lithium iron phosphate and the abundance of earth elements (Fe and P), traditional recycling processes may not be the best choice for processing waste lithium iron phosphate batteries, and more sustainable recycling processes are needed.
[0003] In recent years, people have proposed a process for directly recovering waste lithium iron phosphate, which directly regenerates waste lithium iron phosphate without destroying its olivine structure, thereby avoiding high energy consumption and complex physical phase dissociation process. China Patent Publication No. CN116926572A discloses a method for electrochemical delithiation and simultaneous lithium insertion to repair and recover lithium iron phosphate positive electrode materials, in which the failed lithium iron phosphate positive electrode sheets are used as anode and cathode respectively, and an aqueous solution electrolytic cell is formed with a DC power supply and an electrolyte; after electrolysis, the anode undergoes a delithiation reaction and the cathode undergoes a lithium insertion reaction; during the electrolysis process, the electrolyte is slowly stirred to maintain the uniformity of lithium concentration and pH in the solution; then the iron phosphate powder obtained at the anode and the lithium iron phosphate powder after the cathode is repaired by lithium insertion are collected; the iron phosphate is further recovered by a wet process, and the lithium iron phosphate powder is vacuum calcined to obtain a regenerated lithium iron phosphate material. This method has a complex process, a lengthy process, and is difficult to industrialize. Therefore, it is necessary to develop a method for repairing and regenerating waste lithium iron phosphate with a simple process and easier industrialization. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and seek a method for repairing and regenerating waste lithium iron phosphate positive electrode materials to solve the technical problems of complex process, lengthy process and difficult industrialization in the existing process of repairing and regenerating lithium iron phosphate positive electrode materials.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for repairing and regenerating waste lithium iron phosphate positive electrode materials, the method comprising the following steps:
[0007] (1) Pretreatment: The waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheets are collected, and then calcined in an oxygen-free environment to obtain waste lithium iron phosphate powder;
[0008] (2) Regeneration process: the waste lithium iron phosphate powder, lithium source and dopamine obtained in step (1) are added to a Tris-hydrochloric acid buffer solution, placed under ultraviolet light, stirred at room temperature, and then filtered and dried to obtain a repaired lithium iron phosphate material; under the protection of an inert gas, the repaired lithium iron phosphate material is subjected to a heat treatment to allow the material to be embedded with lithium and the surface to be carbonized to obtain a regenerated lithium iron phosphate material.
[0009] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0010] As a preferred technical solution of the present invention, the temperature of oxygen-free roasting in the pretreatment process of step (1) is 200-600° C., preferably 400° C.; the time of oxygen-free roasting is 1-3 hours, preferably 2 hours;
[0011] Furthermore, the lithium source in the regeneration process of step (2) is any one of lithium chloride, lithium sulfate, lithium carbonate, lithium nitrate, lithium hydroxide, lithium acetate, or a combination of any two thereof, and the addition amount is 10 to 30 wt%;
[0012] Furthermore, the dosage of dopamine and Tris-HCl buffer in the regeneration process of step (2) is 1 to 5 mg / mL;
[0013] Furthermore, the stirring time at room temperature during the regeneration process of step (2) is 3 to 24 hours;
[0014] Furthermore, the heat treatment temperature of the repaired lithium iron phosphate material in step (2) is 600-900° C. and the time is 5-8 hours;
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The present invention realizes efficient repair of lithium iron anti-site defects in waste lithium iron phosphate by room temperature repair, which greatly reduces energy consumption and production costs;
[0017] (2) The method of the present invention is simple in process, easy to operate, and has strong universality. It can achieve efficient regeneration of waste lithium iron phosphate positive electrode materials and is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1It is an XRD comparison chart of the regenerated lithium iron phosphate, waste lithium iron phosphate and commercial lithium iron phosphate standard spectrum in Example 1 of the present invention.
[0019] Figure 2 It is a SEM picture of waste lithium iron phosphate obtained by pretreatment of the present invention.
[0020] Figure 3 This is a SEM image of the regenerated lithium iron phosphate in Example 1 of the present invention.
[0021] Figure 4 This is a TEM image of the regenerated lithium iron phosphate in Example 1 of the present invention.
[0022] Figure 5 It is a comparison chart of the charge and discharge performance of lithium-ion batteries made of regenerated lithium iron phosphate and waste lithium iron phosphate at a rate of 0.1C in Example 1 of the present invention.
[0023] Figure 6 It is a comparison chart of the rate performance of lithium-ion batteries made of regenerated lithium iron phosphate and waste lithium iron phosphate in Example 1 of the present invention.
[0024] Figure 7 It is a comparison chart of the cycle performance of lithium-ion batteries made of regenerated lithium iron phosphate and waste lithium iron phosphate in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] In order to better illustrate the present invention and facilitate understanding of the technical solution, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0026] Embodiment 1:
[0027] (1) First, the waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheet is collected, and then calcined at 400° C. for 2 h in an oxygen-free environment to obtain the waste lithium iron phosphate powder;
[0028] (2) Take 2g of waste lithium iron phosphate powder, lithium hydroxide with a mass fraction of 15wt.%, and 2mg / mL of dopamine, add them into 50mL of Tris-hydrochloric acid buffer, place it under 254&365nm ultraviolet light, stir it at room temperature for 12h, and then filter and dry it to obtain the repaired lithium iron phosphate material; under the protection of argon gas, heat treat the repaired lithium iron phosphate material at 700℃ for 5h to embed lithium in the material and carbonize the surface to obtain regenerated lithium iron phosphate material.
[0029] Embodiment 2-4:
[0030] Except for the different amount of lithium hydroxide added, the other aspects of Example 2-4 are the same as Example 1.
[0031] (1) First, the waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheet is collected, and then calcined at 400° C. for 2 h in an oxygen-free environment to obtain the waste lithium iron phosphate powder;
[0032] (2) Take 2 g of waste lithium iron phosphate powder, lithium hydroxide with a mass fraction of 10 wt.% (Example 2), 20 wt.% (Example 3), and 30 wt.% (Example 4), and 2 mg / mL of dopamine, add them to 50 mL of Tris-hydrochloric acid buffer, place it under 254 & 365 nm ultraviolet light, stir it at room temperature for 12 hours, and then filter and dry it to obtain the repaired lithium iron phosphate material; under the protection of argon gas, the repaired lithium iron phosphate material is heat treated at 700° C. for 5 hours to embed lithium in the material and carbonize the surface to obtain a regenerated lithium iron phosphate material.
[0033] Embodiment 5-6:
[0034] Except for the different amount of dopamine added, all other aspects of Example 5-6 are the same as Example 1.
[0035] (1) First, the waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheet is collected, and then calcined at 400° C. for 2 h in an oxygen-free environment to obtain the waste lithium iron phosphate powder;
[0036] (2) Take 2 g of waste lithium iron phosphate powder, lithium hydroxide with a mass fraction of 15 wt.%, 1 mg / mL (Example 5), 3 mg / mL (Example 6) of dopamine and add them to 50 mL of Tris-hydrochloric acid buffer, place it under 254 & 365 nm ultraviolet light, stir it at room temperature for 12 hours, and then filter and dry it to obtain the repaired lithium iron phosphate material; under the protection of argon gas, the repaired lithium iron phosphate material is heat treated at 700 ° C for 5 hours to embed lithium in the material and carbonize the surface to obtain a regenerated lithium iron phosphate material.
[0037] Embodiment 7-9:
[0038] Except for the stirring time at room temperature, the other aspects of Examples 7-9 are the same as those of Example 1.
[0039] (1) First, the waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheet is collected, and then calcined at 400° C. for 2 h in an oxygen-free environment to obtain the waste lithium iron phosphate powder;
[0040] (2) Take 2 g of waste lithium iron phosphate powder, lithium hydroxide with a mass fraction of 15 wt.%, and 2 mg / mL of dopamine, add them to 50 mL of Tris-hydrochloric acid buffer, place it under 254 & 365 nm ultraviolet light, stir at room temperature for 6 h (Example 7), 9 h (Example 8), and 15 h (Example 9), and then filter and dry to obtain the repaired lithium iron phosphate material; under the protection of argon gas, the repaired lithium iron phosphate material is heat treated at 700 ° C for 5 h to embed lithium in the material and carbonize the surface to obtain a regenerated lithium iron phosphate material.
[0041] Embodiment 10-12:
[0042] Except for the heat treatment temperature, all other aspects of Examples 10-12 are the same as Example 1.
[0043] (1) First, the waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheet is collected, and then calcined at 400° C. for 2 h in an oxygen-free environment to obtain the waste lithium iron phosphate powder;
[0044] (2) Take 2g of waste lithium iron phosphate powder, lithium hydroxide with a mass fraction of 15wt.%, and 2mg / mL of dopamine, add them to 50mL of Tris-hydrochloric acid buffer, place it under 254&365nm ultraviolet light, stir at room temperature for 12h, and then filter and dry to obtain the repaired lithium iron phosphate material; under the protection of argon gas, the repaired lithium iron phosphate material is heat treated at 600℃ (Example 10), 800℃ (Example 11), and 900℃ (Example 12) for 5h to embed lithium in the material and carbonize the surface to obtain regenerated lithium iron phosphate material.
[0045] Embodiment 13-15:
[0046] Except for the heat treatment temperature, all other aspects of Examples 13-15 are the same as Example 1.
[0047] (1) First, the waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheet is collected, and then calcined at 400° C. for 2 h in an oxygen-free environment to obtain the waste lithium iron phosphate powder;
[0048] (2) Take 2g of waste lithium iron phosphate powder, 15wt.% lithium hydroxide, and 2mg / mL dopamine and add them to 50mL Tris-hydrochloric acid buffer, place it under 254&365nm ultraviolet light, stir it at room temperature for 12h, and then filter and dry it to obtain the repaired lithium iron phosphate material; under argon gas protection, the repaired lithium iron phosphate material is heat treated at 800℃ for 6h (Example 13), 7h (Example 14), and 8h (Example 15) to make the material embedded with lithium and carbonize the surface to obtain regenerated lithium iron phosphate material.
[0049] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials used in the present invention, addition of auxiliary raw materials, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for repairing and regenerating waste lithium iron phosphate positive electrode materials, characterized in that: The method comprises the following steps: (1) Pretreatment: The waste lithium iron phosphate battery is completely discharged in a 5% NaCl (w / v) solution, disassembled, separated, and the waste lithium iron phosphate positive electrode sheets are collected, and then calcined in an oxygen-free environment to obtain waste lithium iron phosphate powder; (2) Regeneration process: the waste lithium iron phosphate powder, lithium source and dopamine obtained in step (1) are added to a Tris-hydrochloric acid buffer solution, placed under ultraviolet light, stirred at room temperature, and then filtered and dried to obtain a repaired lithium iron phosphate material; under the protection of an inert gas, the repaired lithium iron phosphate material is subjected to a heat treatment to allow the material to be embedded with lithium and the surface to be carbonized to obtain a regenerated lithium iron phosphate material.
2. The method according to claim 1, characterized in that In the pretreatment process of step (1), the temperature of oxygen-free roasting is 200-600° C., and the time of oxygen-free roasting is 1-3 hours.
3. The method according to claim 1, characterized in that The lithium source in the regeneration process of step (2) is any one of lithium chloride, lithium sulfate, lithium carbonate, lithium nitrate, lithium hydroxide, and lithium acetate, or a combination of any two of them, and the added amount is 10 to 30 wt%.
4. The method according to claim 1, characterized in that The dosage of dopamine and Tris-hydrochloric acid buffer in the regeneration process of step (2) is 1-5 mg / mL.
5. The method according to claim 1, characterized in that The ultraviolet lamp irradiation intensity in the regeneration process of step (2) is 100-400nm.
6. The method according to claims 1-5, characterized in that: The stirring time at room temperature during the regeneration process of step (2) is 3 to 24 hours.
7. The method according to any one of claims 1 to 6, characterized in that: The heat treatment temperature of the repaired lithium iron phosphate material in step (2) is 600-900° C. and the time is 5-8 hours.
8. The method according to any one of claims 1 to 7 is used to repair and regenerate waste lithium iron phosphate positive electrode materials.
Citation Information
Patent Citations
Repair and regeneration method of lithium iron phosphate positive electrode material in waste batteries
CN110277602A
Direct regeneration method of waste lithium iron phosphate positive electrode material
CN114744315A
Repairing and regenerating method of waste lithium iron phosphate battery positive electrode material
CN116902953A
Recycling and reconditioning of battery electrode materials
US9484606B1
Method for recycling spent lithium iron phosphate batteries
WO2023245898A1
Cited By
Lignin illumination assistance-based direct regeneration method of waste lithium iron phosphate positive electrode material, regenerated lithium iron phosphate positive electrode material and application of regenerated lithium iron phosphate positive electrode material
CN122177992A
A method for directly regenerating waste lithium iron phosphate positive electrode material based on lignin light-assisted, regenerated lithium iron phosphate positive electrode material and application
CN122177992B
Regenerated lithium iron phosphate positive electrode sheet and lithium iron phosphate battery
WO2026114329A1