Cellulose-based hard carbon negative electrode material and preparation method and application thereof

By adsorbing cellulose into foam carbon and combining it with oxidation treatment and high-temperature carbonization, a high-efficiency cellulose-based hard carbon anode material was prepared. This solved the problems of low residual carbon content and uncontrollable pre-oxidation of cellulose-based hard carbon, enabling high-capacity and high-efficiency sodium-ion battery applications, and has industrialization prospects.

CN118983440AInactive Publication Date: 2024-11-19TAIAN FARADAY ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411054484.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Cellulose-based hard carbon materials have low residual carbon content and uncontrollable pre-oxidation processes, resulting in high costs and difficulty in industrialization.

Method used

Cellulose-based hard carbon anode materials were prepared by using foamed carbon adsorbed cellulose as a precursor and through oxidation treatment and high-temperature carbonization, while controlling the oxidation process and forming a closed pore structure.

Benefits of technology

It improves the specific surface area and initial coulombic efficiency of hard carbon materials, reduces costs, and has the potential for large-scale industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983440A_ABST
    Figure CN118983440A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery manufacturing, and particularly relates to a cellulose-based hard carbon negative electrode material and a preparation method and application thereof, the cellulose-based hard carbon negative electrode material is prepared by taking cellulose as a carbon source precursor, adsorbing the cellulose by foamy carbon, and then performing oxidation treatment and high-temperature carbonization treatment. Cellulose is adsorbed in foamy carbon for oxidation treatment, and the foamy carbon can isolate cellulose and prevent mass agglomeration of cellulose, so that heat in the oxidation process is not uncontrollable. After the cellulose is adsorbed on the foamy carbon, the internal pore diameter of the foamy carbon is filled, the formation of closed pores is facilitated after oxidation and high-temperature carbonization, the specific surface area of the obtained hard carbon is small, and the first effect and the capacity of the hard carbon material are obviously improved. Therefore, when the material is applied as a sodium ion battery negative electrode material, high capacity and first coulombic efficiency are shown, and the feasibility of large-scale production is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery manufacturing, and in particular relates to a cellulose-based hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy vehicles, lithium-ion batteries have become very important. Sodium has a higher abundance in the earth's crust, accounting for about 2.64% of the earth's crust reserves, and is widely distributed around the world. The raw material sodium carbonate is easy to refine and its price is much lower than lithium carbonate. The overall performance of sodium batteries is close to that of lithium batteries, with slightly lower energy density, but outstanding low temperature, safety and rate performance. Therefore, sodium-ion batteries have become a supplementary substitute for lithium-ion batteries and have attracted the attention of researchers.

[0003] Hard carbon has become an extremely excellent negative electrode material for sodium ion batteries due to its excellent performance and low cost. The preparation of hard carbon materials is usually obtained by pyrolysis of various carbon-containing precursors. Different precursors will lead to different electrochemical properties of hard carbon materials. According to the source of the precursor, it can be mainly divided into three types of hard carbon: resin-based (phenolic resin, epoxy resin, polyfurfuryl alcohol, etc.) hard carbon, asphalt-based (coal tar asphalt, petroleum asphalt, natural asphalt, etc.) hard carbon, biomass-based (cellulose, lignin, starch, etc.) hard carbon. Biomass-based hard carbon such as cellulose has the advantages of wide range of raw materials, low cost, environmental friendliness, and wide sources. However, the carbon residue of cellulose carbonization is only 10%, which leads to increased costs. Pre-oxidation is an effective strategy to increase the carbon residue. In addition, the cellulose oxidation process is an exothermic reaction, and industrialization cannot be controlled. How to reduce the exothermic reaction kinetics to achieve commercialization has become a difficulty. Summary of the invention

[0004] The purpose of the present invention is to provide a cellulose-based hard carbon negative electrode material and a preparation method and application thereof. In order to solve the problems of low residual carbon content and uncontrollable pre-oxidation of the hard carbon precursor cellulose, cellulose is used as a carbon source precursor, and foam carbon is used to adsorb cellulose. The cellulose-based hard carbon negative electrode material is prepared by oxidation treatment and high-temperature carbonization. It is used as a negative electrode material for sodium ion batteries, showing high capacity and first coulombic efficiency, and has prospects for large-scale industrialization.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] The present invention provides a method for preparing a cellulose-based hard carbon negative electrode material, comprising the following steps:

[0007] The method uses cellulose as a carbon source precursor, adopts an adsorption template to adsorb cellulose, and then undergoes oxidation treatment and high-temperature carbonization treatment to obtain the product.

[0008] Furthermore, the mass concentration of the cellulose is 5-15%.

[0009] Furthermore, the mass ratio of the cellulose to the adsorption template is 1:0.5-5.

[0010] Furthermore, the adsorption template is foamed carbon.

[0011] Furthermore, a drying step is included before the oxidation treatment.

[0012] Furthermore, the temperature during the oxidation treatment is 240-300° C., and the time of the oxidation treatment is 1-6 hours.

[0013] Furthermore, the temperature during the high-temperature carbonization treatment is 1350-1550°C, the heating rate during the high-temperature carbonization treatment is 0.5-10°C / minute, and the carbonization atmosphere during the high-temperature carbonization treatment is any one of N2, He, Ar, NH3, H2-Ar, H2-N2 and H2-He.

[0014] Furthermore, the cellulose is any one of hydroxymethyl cellulose, hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl cellulose and carboxymethyl cellulose.

[0015] The present invention also provides a cellulose-based hard carbon negative electrode material, wherein the cellulose-based hard carbon negative electrode material has a -1 At a current density of 350 mAh g -1 Above, the Coulomb efficiency is greater than 91%.

[0016] The present invention also provides an application of a cellulose-based hard carbon negative electrode material in the preparation of a sodium ion battery.

[0017] The beneficial effects of the present invention are:

[0018] The present invention uses cellulose as a carbon source precursor, uses foamed carbon to adsorb cellulose, and prepares a hard carbon negative electrode material through oxidation treatment and high-temperature carbonization. The carbonized product is used as a negative electrode material for a sodium ion battery, which exhibits high capacity and first coulombic efficiency. Among them, the cellulose is adsorbed in the foamed carbon for oxidation treatment, and the foamed carbon can isolate the cellulose to prevent it from agglomerating in large quantities, so that the heat of the oxidation process is not uncontrollable. And after the cellulose is adsorbed on the foamed carbon, the internal pore size of the foamed carbon is filled, and oxidation and high-temperature carbonization contribute to the formation of closed pores. The obtained hard carbon has a small specific surface area, and the first efficiency and capacity of the hard carbon material are significantly improved. Moreover, cellulose is widely available, low in cost, and the hard carbon synthesis process is simple and easy to implement in production, which has industrial prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 The diffraction XRD pattern of the cellulose-based hard carbon negative electrode material prepared in Example 1;

[0021] Figure 2 This is the electrochemical performance diagram of the cellulose-based hard carbon negative electrode material prepared in Example 1. DETAILED DESCRIPTION

[0022] The embodiments of the present invention are described in detail below, and the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. If specific techniques or conditions are not specified in the embodiments, they are carried out according to the techniques or conditions described in the literature in this area or according to the product specifications. If the manufacturers of reagents or instruments are not specified, they are all conventional products that can be obtained commercially.

[0023] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0024] The cellulose-based hard carbon negative electrode material of the present invention uses cellulose with a mass concentration of 5-15% as a carbon source precursor, and the cellulose and foam carbon are adsorbed by the foam carbon in a ratio of 1:0.5-5, and dried, and then oxidized at 240-300°C for 1-6 hours, and then subjected to high-temperature carbonization treatment to obtain the obtained material.

[0025] The cellulose is any one of hydroxymethyl cellulose, hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl cellulose and carboxymethyl cellulose.

[0026] The high-temperature carbonization temperature during the high-temperature carbonization treatment is 1350-1550°C, the heating rate during the carbonization process is 0.5-10°C / minute, and the carbonization atmosphere is any one of N2, He, Ar, NH3, H2-Ar, H2-N2 and H2-He.

[0027] The following examples are used to further illustrate the present invention, but are not intended to limit the present invention.

[0028] Example 1

[0029] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 1 of the present invention has the following specific implementation scheme:

[0030] Take 1g of dry hydroxymethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 240℃ at 5℃ per minute, oxidize it for 6 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. The diffraction XRD pattern of the cellulose-based hard carbon negative electrode material is shown in Figure 1 shown.

[0031] The sodium ion battery was electrochemically tested using the cellulose hard carbon anode material prepared by the above preparation method as the anode material, sodium metal sheet as the cathode, 1M NaFP6 dissolved in DMC:EMC:EC (1:1:1) as the electrolyte, and celgard 2400 as the separator. The electrochemical performance of the cellulose-based hard carbon anode material is shown in the figure. Figure 2 As shown, this cellulose hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 352.3 mAh g -1 , the first coulombic efficiency is 91.5%.

[0032] Example 2

[0033] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 2 of the present invention has the following specific implementation scheme:

[0034] Take 1g of dry hydroxyethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 240℃ at 5℃ per minute, oxidize it for 6 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 351.6 mAh g -1 , the first coulombic efficiency is 91.6%.

[0035] Example 3

[0036] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 3 of the present invention has the following specific implementation scheme:

[0037] Take 1g of dry methyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with air atmosphere, heat it to 240℃ at 5℃ per minute, oxidize it for 6 hours, change to nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material has a high conductivity at 35mAg -1 The first discharge capacity at the current density is 352.5 mAh g -1 , the first coulombic efficiency is 91.6%.

[0038] Example 4

[0039] The method for preparing the cellulose-based hard carbon negative electrode material provided in Example 4 of the present invention has the following specific implementation scheme:

[0040] Take 1g of dry ethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with air atmosphere, heat it to 240℃ at 5℃ per minute, oxidize it for 6 hours, change to nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material has a high conductivity at 35mAg -1 The first discharge capacity at the current density is 353.2 mAh g -1 , the first Coulombic efficiency is 91.7%.

[0041] Example 5

[0042] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 5 of the present invention has the following specific implementation scheme:

[0043] Take 1g of dry hydroxypropyl methylcellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 240℃ at 10℃ per minute, oxidize it for 6 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 355.3 mAh g -1 , the first Coulombic efficiency is 91.8%.

[0044] Example 6

[0045] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 6 of the present invention has the following specific implementation scheme:

[0046] Take 1g of dry hydroxypropyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 240℃ at 10℃ per minute, oxidize it for 6 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 354.7 mAh g -1 , the first Coulombic efficiency was 91.9%.

[0047] Example 7

[0048] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 7 of the present invention has the following specific implementation scheme:

[0049] Take 1.5g of dry hydroxypropyl methylcellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 240℃ at 5℃ per minute, oxidize it for 6 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 3℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 356.2 mAh g -1 , the first coulombic efficiency is 92.1%.

[0050] Example 8

[0051] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 8 of the present invention has the following specific implementation scheme:

[0052] Take 1g of dry hydroxymethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with air atmosphere, heat it to 250℃ at 5℃ per minute, oxidize it for 5 hours, change to nitrogen atmosphere, heat it to 1450℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 354.2 mAh g -1 , the first Coulombic efficiency is 91.7%.

[0053] Example 9

[0054] The preparation method of the cellulose-based hard carbon negative electrode material provided in Example 9 of the present invention has the following specific implementation scheme:

[0055] Take 1g of dry hydroxymethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 260℃ at 5℃ per minute, oxidize it for 4 hours, change to a nitrogen atmosphere, heat it to 1500℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 355.8 mAh g -1 , the first coulombic efficiency is 92.0%.

[0056] Example 10

[0057] The method for preparing the cellulose-based hard carbon negative electrode material provided in Example 10 of the present invention has the following specific implementation scheme:

[0058] Take 1g of dry hydroxymethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 270℃ at 5℃ per minute, oxidize it for 4 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 350.6 mAh g -1 , the first coulombic efficiency is 91.6%.

[0059] Embodiment 11

[0060] The method for preparing the cellulose-based hard carbon negative electrode material provided in Example 11 of the present invention has the following specific implementation scheme:

[0061] Take 1g of dry hydroxymethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 280℃ at 5℃ per minute, oxidize it for 3 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 2.5℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 350.1 mAh g -1 , the first coulombic efficiency is 91.5%.

[0062] Example 12

[0063] The method for preparing the cellulose-based hard carbon negative electrode material provided in Example 12 of the present invention has the following specific implementation scheme:

[0064] Take 1g of dry hydroxyethyl cellulose and place it in 10mL of water and stir at 100℃ to form a solution. Put 2g of foam carbon into the solution to adsorb cellulose and dry it at 100℃. Place the dried compound in a tubular furnace with an air atmosphere, heat it to 260℃ at 5℃ per minute, oxidize it for 4 hours, change to a nitrogen atmosphere, heat it to 1400℃ at 2℃ per minute and keep it warm for 3 hours. Cool it to room temperature to obtain a cellulose-based hard carbon negative electrode material. This cellulose-based hard carbon negative electrode material is 35mAg -1 The first discharge capacity at the current density is 356.6 mAh g -1 , the first coulombic efficiency is 92.1%.

[0065] Comparative Example 1

[0066] Comparative Example 1 provides a conventional method for preparing a cellulose-based hard carbon negative electrode material:

[0067] 100g of dried cellulose was placed in a tubular furnace in an Ar atmosphere, and the temperature was raised to 1400℃ at 2℃ per minute and kept at that temperature for 3 hours. After cooling to room temperature, a cellulose-based hard carbon negative electrode material was obtained. -1 The first discharge capacity at the current density is 302.4 mAh g -1 , the first coulombic efficiency was 88.7% and the yield was 8.9%.

[0068] Through comparison, it is obvious that the cellulose-based hard carbon negative electrode materials prepared in Examples 1-12 of the present application have higher first discharge specific capacity and higher first coulombic efficiency than those in Comparative Example 1. In addition, cellulose is widely available and inexpensive, and the hard carbon synthesis process is simple and easy to implement in production, which has industrial prospects.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be covered by the scope of the claims of the present invention.

Claims

1. A method for preparing a cellulose-based hard carbon negative electrode material, characterized in that: The following steps are involved: The method uses cellulose as a carbon source precursor, adopts an adsorption template to adsorb cellulose, and then undergoes oxidation treatment and high-temperature carbonization treatment to obtain the product.

2. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The mass concentration of the cellulose is 5-15%.

3. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of the cellulose to the adsorption template is 1:0.5-5.

4. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The adsorption template is foamed carbon.

5. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The method further includes a drying step before the oxidation treatment.

6. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The temperature during the oxidation treatment is 240-300° C., and the time of the oxidation treatment is 1-6 hours.

7. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The high-temperature carbonization treatment temperature is 1350-1550°C, the heating rate of the high-temperature carbonization treatment is 0.5-10°C / minute, and the carbonization atmosphere during the high-temperature carbonization treatment is any one of N2, He, Ar, NH3, H2-Ar, H2-N2 and H2-He.

8. The method for preparing a cellulose-based hard carbon negative electrode material according to claim 1, characterized in that: The cellulose is any one of hydroxymethyl cellulose, hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose, hydroxypropyl cellulose and carboxymethyl cellulose.

9. The cellulose-based hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The cellulose-based hard carbon negative electrode material has a -1 At a current density of 350 mAh g -1 Above, the Coulomb efficiency is greater than 91%.

10. Use of the cellulose-based hard carbon negative electrode material as claimed in claim 8 in the preparation of sodium ion batteries.