Internal heating battery and preparation method thereof
By designing an internal heating battery in a lithium battery and using an electrothermal layer for internal heating, the problems of slow dynamics and uneven temperature in a low-temperature environment are solved, rapid and uniform heating is achieved, and the thermal stability of the diaphragm is improved, and the thermal stability of the diaphragm is improved. The low temperature performance and safety of the battery.
Patent Information
- Application Number
- CN202410894994.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-19
AI Technical Summary
Lithium batteries have slow dynamics in low temperature environments and intensified polarization, resulting in a significant attenuation of energy density and power density. The existing thermal management systems have problems such as low heat exchange efficiency, uneven temperature and insufficient safety.
Design an internal heating battery, using a bare cell and an electrothermal layer, which consists of a conductive electrode and an electrothermal body layer, and is connected to the electrothermal layer through a conductive electrode to form an independent electrothermal layer. The layer is located between the positive and negative electrodes, and is heated internally using an electrothermal layer, assembled in laminate or winding, and sealed through an aluminum-plastic film bag.
It achieves rapid and uniform heating of the battery cell, significantly improves the thermal stability of the diaphragm and the safety of the battery, and improves the performance of the battery in low temperature environments.
Smart Images

Figure CN118983581A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium batteries and relates to the design of an internal heating battery and a preparation method thereof. Background Art
[0002] Lithium batteries need to work at a suitable temperature, usually 15-35°C. At low temperatures, the battery's dynamics are slow and polarization is aggravated, resulting in a significant decrease in energy density and power density. Poor low-temperature performance severely limits the application scenarios of lithium batteries, including winter, high altitudes, high latitudes, deep sea and space. In traditional battery structures, including consumer batteries, power batteries and energy storage batteries, thermal management systems are usually used to heat the battery cells.
[0003] There are air-type, liquid-type, heat pipe-type and phase change material-type thermal management systems. The air-type thermal management system has a simple structure, but the heat exchange efficiency is low; the liquid-type thermal management system is the current mainstream solution, which has high heat exchange efficiency, but there is a risk of leakage and may cause a short circuit in the battery; the heat pipe-type thermal management system has high heat exchange efficiency, but cannot guarantee uniform temperature distribution; the phase change material-type thermal management system can ensure temperature uniformity, but the heat exchange efficiency is low and it is difficult to package (Yu Z, et al. Journal of Energy Storage, 2023, 62: 106827.). Therefore, the development of a simple and efficient thermal management system is urgently needed to maximize the low-temperature performance of lithium batteries.
[0004] At present, the heating elements of the thermal management system are all located outside the battery cell. In the early stage of heating, a certain temperature gradient will be formed inside the battery cell, and it takes a certain amount of time for the temperature inside the battery cell to reach uniformity (Nasajpour-Esfahani N, et al. Journal of Energy Storage, 2023, 63: 107061.). It is expected that fast and uniform heating can be achieved by heating the battery cell internally, but it is still rarely reported. Summary of the invention
[0005] In view of the above problems existing in the prior art, the object of the present invention is to provide a design of an internal heating battery and a method for preparing the same.
[0006] In order to solve the above problems, the present invention provides an internally heated battery, comprising a bare cell, an electrolyte and a shell; the bare cell immersed in the electrolyte is sealed in the shell (aluminum-plastic film bag), the bare cell comprises a positive electrode, a negative electrode, a diaphragm, an electrothermal layer and a tab, the diaphragm comprises a first diaphragm and a second diaphragm, and the tabs comprise a first tab, a second tab, a third tab and a fourth tab;
[0007] The positive electrode, the first diaphragm, the electrothermal layer, the second diaphragm, and the negative electrode are arranged in sequence; the first electrode tab is electrically connected to the positive electrode, the second electrode tab is electrically connected to the negative electrode, and the third electrode tab and the fourth electrode tab are electrically connected to both ends of the electrothermal layer, respectively.
[0008] Therefore, the electrothermal layer is located between the positive electrode and the negative electrode, and is electronically insulated from the positive and negative electrodes by the first separator and the second separator.
[0009] As an improvement of the internally heated battery of the present invention: the bare cell assembly is performed by lamination or winding.
[0010] As a further improvement of the internally heated battery of the present invention: the electrothermal layer has electronic conductivity and ionic conductivity.
[0011] As a further improvement of the internally heated battery of the present invention: the electrothermal layer is composed of an electrothermal body layer and a conductive electrode; conductive electrodes are respectively arranged at both ends of the electrothermal layer, and the third pole tab and the fourth pole tab are respectively connected to corresponding conductive electrodes.
[0012] The present invention also provides a method for preparing the internal heating battery, comprising the following steps:
[0013] 1) Preparation of electrothermal layer:
[0014] The electrothermal layer is composed of an electrothermal body layer and a conductive electrode;
[0015] Coating a slurry of an electrothermal material (double conductive slurry) on the entire surface of the first diaphragm facing the second diaphragm, and then drying (drying at 60 to 80° C. for 30 to 180 minutes) to form an electrothermal bulk layer with a thickness of 1 to 10 μm (preferably 6 to 8 μm);
[0016] The electrothermal material is composed of ionic conductive agent, electronic conductive agent I and binder I with mass contents of 84-86%, 9-11% and 4.5-5.5% respectively (obtained after slurry mixing);
[0017] Note: The surface areas of the electrothermal layer and the first diaphragm are equal (i.e., the sizes of the two are consistent);
[0018] A slurry of a conductive electrode material (conductive slurry) is coated on the left and right ends of the electrothermal body layer respectively, and then dried (at 60 to 80° C. for 30 to 180 minutes), thereby forming two strip-shaped conductive electrodes located on the electrothermal body layer;
[0019] The conductive electrode material is composed of an electronic conductive agent II and a binder II with mass contents of 89-91% and 9-11% respectively;
[0020] 2) Cutting a second diaphragm having a surface area consistent with that of the first diaphragm (i.e., the two diaphragms have the same size);
[0021] 3) Pole cutting:
[0022] The surface area of the positive electrode sheet is smaller than that of the negative electrode sheet, and the surface area of the negative electrode sheet is smaller than that of the first separator;
[0023] 4) Bare battery cell assembly:
[0024] The bare cell assembly adopts a lamination or winding process, and the basic unit of the bare cell is a positive electrode sheet-a first diaphragm (bare diaphragm)-an electrothermal layer-a second diaphragm (bare diaphragm)-a negative electrode sheet;
[0025] 5) Ear welding:
[0026] The positive electrode sheet is welded with the first pole ear, the negative electrode sheet is welded with the second pole ear, and the third pole ear and the fourth pole ear are respectively connected to the conductive electrode of the electric heating layer; and a bare battery cell with the pole ears welded thereon is obtained;
[0027] 6) The bare battery cell with the tabs welded thereto is subjected to subsequent conventional packaging processing to obtain an internally heated battery.
[0028] As an improvement of the preparation method of the internal heating battery of the present invention:
[0029] The ion conductive agent is lithium aluminum titanium phosphate, the electronic conductive agent I is carbon nanotubes, and the binder I is polyvinylidene fluoride;
[0030] The electronic conductive agent II is silver nanowire, and the binder II is polyvinylidene fluoride.
[0031] As a further improvement of the preparation method of the internal heating battery of the present invention:
[0032] The electrothermal material is composed of an ionic conductive agent, an electronic conductive agent I and a binder I in a mass ratio of 85:10:5 (obtained after slurry mixing);
[0033] The conductive electrode material is composed of an electronic conductive agent II and a binder II in a mass ratio of 90:10.
[0034] As a further improvement of the preparation method of the internal heating battery of the present invention:
[0035] Subsequent packaging processing includes bagging and packaging, vacuum baking, liquid injection, degassing and packaging, and standing;
[0036] The details are as follows:
[0037] 6.1) Bagging and packaging: Put the bare battery cell with the tabs welded into an aluminum-plastic film bag, and package the top edge and one side edge with the tabs;
[0038] 6.2) Vacuum baking: Bake the packed cells under vacuum at a temperature of 60-90°C for 4-6 hours;
[0039] 6.3) Injection:
[0040] injecting electrolyte into the baked battery cell;
[0041] 6.4) Degassing and packaging:
[0042] Degas the battery cell after liquid injection and package the other side;
[0043] 6.5) Stand still:
[0044] The packaged soft-pack batteries are placed at room temperature or high temperature, the temperature is 20-80°C, and the time is 4-24h.
[0045] As a further improvement of the preparation method of the internal heating battery of the present invention:
[0046] The first separator and the second separator are both polyolefin porous membranes, and the polyolefin porous membranes include polyethylene porous membranes, polypropylene porous membranes, and the like.
[0047] As a further improvement of the preparation method of the internal heating battery of the present invention:
[0048] The electrothermal material slurry (double conductive slurry) is composed of the electrothermal material with a mass concentration of 30-35% and a solvent (N-methylpyrrolidone) as the balance;
[0049] The slurry of the conductive electrode material (conductive slurry) is composed of the conductive electrode material at a mass concentration of 4 to 6% and a solvent (N-methylpyrrolidone) as the balance.
[0050] The present invention arranges an independent electric heating layer between the positive and negative electrodes of the battery, and leads out the third and fourth electrodes.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] 1) The battery provided by the present invention can be heated between the positive and negative electrodes inside the battery core through the electrothermal layer, with a faster heating speed and more uniform temperature distribution.
[0053] 2) The electrothermal layer provided by the present invention can significantly improve the thermal stability of the diaphragm, thereby improving the safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.
[0055] Figure 1This is a schematic diagram of the structure of a single-layer laminated internal heating battery prepared in Example 1;
[0056] Figure 2 The electrothermal layer prepared in Example 1; the upper figure (surface) represents the surface, and the lower figure (section) represents the interface;
[0057] Figure 3 Schematic diagram of the electrothermal test in Example 1;
[0058] Figure 4 The electrothermal curve of the electrothermal layer recorded by the thermocouple in Example 1;
[0059] Figure 5 The temperature distribution of the electrothermal layer in the transverse and longitudinal directions recorded by the thermal imager in Example 1;
[0060] Figure 5 Middle: a is the thermal imaging picture of the electrothermal layer in the initial state (no external voltage), bf are the temperature distribution curves of the thermal imaging pictures of the electrothermal layer in the horizontal direction (L0) and the vertical direction (L1) under the external voltages of Initial, 15, 20, 25, and 30 V respectively;
[0061] Figure 6 is a differential scanning calorimetry curve of the diaphragm coated with the electric heating layer in Example 1;
[0062] Figure 7 The heat shrinkage of the diaphragm coated with the electrothermal layer in Example 1;
[0063] Figure 8 is the wetting angle of the diaphragm coated with the electrothermal layer in Example 1;
[0064] Fig. 9 This is a schematic diagram of the structure of the electric heating layer prepared in Example 2;
[0065] Fig.10 This is a schematic diagram of the appearance of a multi-layer laminated internal heating battery prepared in Comparative Example 2;
[0066] Fig.11 is the differential scanning calorimetry curve of the bare diaphragm in Comparative Example 1;
[0067] Fig.12 The heat shrinkage of the bare diaphragm in Comparative Example 1;
[0068] Fig.13 is the wetting angle of the bare diaphragm in Comparative Example 1. DETAILED DESCRIPTION
[0069] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:
[0070] The materials used in the present invention can all be obtained in commercial form, for example:
[0071] The main performance parameters of lithium aluminum titanium phosphate are: D50 is 100-300nm; for example, lithium aluminum titanium phosphate with model number MA-EN-SS-0003 sold by CLUDE Corporation can be selected.
[0072] The main performance parameters of carbon nanotubes are: diameter of 7-11 nm; for example, the carbon nanotubes of model MA-EN-CO-0B sold by CLUDE Corporation can be used.
[0073] The first diaphragm and the second diaphragm are both polypropylene porous membranes, and the main performance parameters of the polypropylene porous membranes are: thickness of 25 μm, porosity of 55%; for example, the polypropylene porous membrane model 2500 sold by Celgard Company can be selected;
[0074] The main performance parameters of the silver nanowires are: a diameter of 90 nm; for example, the silver nanowires of 90 nm sold by Zhejiang Kexin New Materials Company can be used.
[0075] The positive electrode sheet is a ternary positive electrode sheet (single-sided coating or double-sided coating); the single-sided surface capacity is 3.03 mAh / cm2, for example, the ternary positive electrode sheets SY3203 and SY3204 of Krud Company can be selected;
[0076] The negative electrode sheet is a graphite negative electrode sheet (single-sided coating or double-sided coating), and the single-sided surface capacity is 3.44mAh / cm2. When it is a single-sided coated graphite negative electrode sheet, for example, the SM0204 graphite negative electrode sheet of Kruder Company can be selected; when it is a double-sided coated graphite negative electrode sheet, for example, the SM0205 graphite negative electrode sheet of Kruder Company can be selected.
[0077] Embodiment 1: A single-layer laminated internal heating battery, the following steps are performed in sequence:
[0078] 1) Preparation of electrothermal layer:
[0079] The electrothermal layer is composed of an electrothermal body layer and a conductive electrode;
[0080] Lithium aluminum titanium phosphate, carbon nanotubes and polyvinylidene fluoride are mixed in a mass ratio of 85:10:5 to form a mixture I. N-methyl pyrrolidone is added to the mixture I and stirred evenly to obtain a dual conductive paste with a mass content of 33% of the mixture I, that is, the solid content of the dual conductive paste is 33%; lithium aluminum titanium phosphate has ionic conductivity, and carbon nanotubes have electronic conductivity.
[0081] The dual conductive slurry was coated onto the entire surface of the first separator (polypropylene porous membrane) with a 35 μm scraper to form a conductive separator wet film with a thickness of 35 μm, and then transferred to a 60°C oven for drying for 1 hour to obtain an electric heating layer body layer (thickness of about 7 μm). Its morphology is as follows Figure 2 . Figure 2 The “Surface” in the figure represents the scanning electron microscope image of the surface, and the “Section” represents the scanning electron microscope image of the cross section.
[0082] The surface areas of the electrothermal layer body layer and the first diaphragm are equal (ie, the sizes of the two are consistent).
[0083] Silver nanowires and polyvinylidene fluoride are mixed at a mass ratio of 90:10 to obtain a mixture II. N-methylpyrrolidone is added to the mixture II and stirred to obtain a conductive paste having a mass content of 5% of the mixture II, that is, a solid content of the conductive paste of 5%;
[0084] The conductive paste is coated on the symmetrical long sides of the electrothermal layer body layer with a screen, thereby forming two strip-shaped (4 mm wide) conductive electrodes located on the electrothermal body layer; then transferred to a 60° C. oven for drying for 1 hour to obtain an electrothermal layer coated with symmetrical silver electrodes (4 mm wide), wherein the electrothermal layer is located on the surface of the first diaphragm;
[0085] 2) Diaphragm cutting:
[0086] The second separator (polypropylene porous membrane) and the first separator provided with the electrothermal layer were cut into 53.2×46.5 mm, respectively; that is, the first separator and the second separator were of the same size.
[0087] 3) Pole cutting:
[0088] The positive electrode sheet is a ternary positive electrode sheet, and the positive electrode sheet is coated on one side; the negative electrode sheet is a graphite negative electrode sheet, and the negative electrode sheet is coated on one side.
[0089] The positive electrode sheet is cut to 49.5×42.0mm, and the negative electrode sheet is cut to 51.0×43.5mm.
[0090] That is, the surface area of the positive electrode sheet is smaller than that of the negative electrode sheet, and the surface area of the negative electrode sheet is smaller than that of the first separator;
[0091] 4) Bare battery cell assembly:
[0092] The bare cell assembly adopts a single-layer lamination process, and the bare cell is stacked (laminated) in the order of positive electrode sheet-first diaphragm-electric heating layer-second diaphragm-negative electrode sheet, that is, the electric heating layer on the first diaphragm faces the second diaphragm as a bare diaphragm; its schematic diagram is as follows Figure 1The centers of the positive electrode sheet, the first diaphragm provided with the electrothermal layer, the second diaphragm, and the negative electrode sheet overlap.
[0093] 5) Ear welding:
[0094] The positive electrode sheet of the bare cell is welded with an aluminum tab (the first tab), and the negative electrode sheet is welded with a nickel tab (the second tab). First, a 4.0×20.0 mm copper foil (5 μm thick) is attached to each of the two silver electrodes of the electrothermal layer, and then the two copper foils are welded to the other two nickel tabs (the third tab and the fourth tab) respectively; a bare cell with tabs welded is obtained, as shown in the schematic diagram. Figure 1 .
[0095] The first pole lug, the second pole lug, the third pole lug, and the fourth pole lug may be located on the same side of the bare battery cell; or they may be located on different sides.
[0096] 6) Perform conventional subsequent packaging on the bare battery cell with the tabs welded to it:
[0097] Including bagging and packaging, vacuum baking, liquid injection, degassing and packaging, standing, and clamping;
[0098] The details are as follows:
[0099] 6.1) Bagging and packaging:
[0100] Select an aluminum-plastic film bag with an opening on the top and both sides, and the size of the aluminum-plastic film bag is larger than the bare battery cell; put the bare battery cell with the electrode tabs welded obtained in step 5) into the aluminum-plastic film bag, at this time, the ends of the first electrode tab, the second electrode tab, the third electrode tab, and the fourth electrode tab are all exposed at the top of the aluminum-plastic film bag. The top and any one side of the aluminum-plastic film bag are packaged.
[0101] 6.2) Vacuum baking: Bake the packed cells in a vacuum environment at a temperature of 85°C for 4 hours;
[0102] 6.3) Injection:
[0103] Inject 0.5 mL of electrolyte into the baked battery cell;
[0104] 6.4) Degassing and packaging:
[0105] Degas the battery cell after injection (air) and encapsulate the other side;
[0106] 6.5) Stand still:
[0107] The packaged soft-pack battery is left to stand at room temperature for 24 hours;
[0108] 6.6) Upper fixture:
[0109] The battery after standing was clamped under a pressure of 0.4 MPa, that is, the clamp only contacted the aluminum-plastic film bag, so that the internal contact of the battery was good.
[0110] Experiment 1: Test of the electrothermal performance of the electrothermal layer:
[0111] According to step 1) of Example 1, a first diaphragm coated with an electrothermal layer was prepared, and then a 2.5×4.5 cm 2 The first diaphragm coated with an electrothermal layer (ie, the front side of the first diaphragm is provided with an electrothermal layer), and the electrothermal layer body layer is 2.5×4.5 cm 2 The two silver electrodes are 2.5×1cm 2 , wherein the portion of the uncoated silver electrode is affixed with a thermocouple on the back (i.e., the reverse side of the first diaphragm is affixed with a thermocouple), and the two silver electrodes are respectively connected to the two poles of a DC power supply, such as Figure 3 shown.
[0112] Connect 15, 20, 25 or 30V DC respectively and record the temperature change of the thermocouple.
[0113] The recorded data is as follows Figure 4 , the temperature of the electrothermal layer tends to stabilize within 90s at a voltage of 15-30V.
[0114] After the temperature of the thermocouple tends to be stable, the temperature distribution on the surface of the electrothermal layer is recorded using a thermal imager.
[0115] The recorded data is as follows Figure 5 The average temperature of the surface of the electrothermal layer is 23°C without external voltage, and at 15V ( Figure 5 c) 20V( Figure 5 d) 25V( Figure 5 e) and 30 V (Fig. f), the temperature distribution in the transverse and longitudinal directions of the surface of the electrothermal layer is uniform, and the average temperatures are approximately 45, 60, 80 and 100 °C, respectively.
[0116] according to Figure 4 and Figure 5 , it can be known that the electrothermal layer has fast, uniform and adjustable heating capabilities.
[0117] Experiment 2: Performance test of the diaphragm coated with an electrothermal layer:
[0118] 1) Thermal stability test:
[0119] The first diaphragm coated with the electrothermal layer prepared in step 1) of Example 1 was tested using a differential scanning calorimeter, with a heating rate of 3° C. / min and nitrogen as the protective gas.
[0120] The recorded data is as follows Figure 6The closed-pore and melting peak temperatures of the diaphragm (the diaphragm coated with the electrothermal layer) were 161.1 and 170.6 °C, respectively, while the closed-pore and melting peak temperatures of the bare diaphragm were 159.5 and 165.5 °C, respectively (data recorded as Fig.11 ).
[0121] The diaphragm coated with the electric heating layer was tested in a constant temperature box at a temperature of 180°C and a holding time of 30 minutes.
[0122] The recorded data is as follows Figure 7 The heat shrinkage of the diaphragm is 25.6%, while the heat shrinkage of the bare diaphragm is 54.5% (the recorded data are as follows Fig.12 ).
[0123] according to Figure 6 and Figure 7 It can be seen that the electrothermal layer improves the thermal stability of the diaphragm.
[0124] 2) Wettability test:
[0125] The diaphragm coated with the electrothermal layer is tested using a contact angle meter. The liquid medium is an electrolyte, and the electrolyte is dropped onto the diaphragm coated with the electrothermal layer.
[0126] The recorded data is as follows Figure 8 The static contact angle of the electrothermal layer is 14.1°, while that of the bare diaphragm is 39.9° (data recorded as Fig.13 ).
[0127] Therefore, it can be understood that the electrothermal layer improves the wettability of the separator.
[0128] In summary, since the electrothermal layer of the present invention has a fast and uniform electrothermal capability, and since it is located inside the battery cell, the battery will inevitably have a faster and more uniform electrothermal capability.
[0129] Embodiment 2: A multi-layer laminated internal heating battery, the following steps are performed in sequence:
[0130] 1) The preparation of the electrothermal layer is the same as step 1) of Example 1;
[0131] 2) Diaphragm cutting:
[0132] The second diaphragm and the first diaphragm provided with the electrothermal layer were cut into 54.0×1005.4 mm, respectively. That is, the first diaphragm and the second diaphragm had the same size.
[0133] 3) Pole cutting:
[0134] The positive electrode sheet is a ternary positive electrode sheet, and the positive electrode sheet is coated on both sides; the negative electrode sheet is a graphite negative electrode sheet, and the negative electrode sheet is coated on one side or on both sides.
[0135] The cutting dimensions of the positive electrode sheet and the negative electrode sheet are the same as those in Example 1.
[0136] 4) Bare battery cell assembly:
[0137] The bare cell assembly adopts the Z-type lamination process. The first diaphragm-electric heating layer-second diaphragm is combined to form a membrane assembly. The membrane assembly is folded in a Z-type manner. Negative and positive electrodes are alternately arranged in the adjacent two-layer membrane assembly. There are 10 negative electrode sheets. The negative electrode sheets at the upper and lower ends are coated on one side, with the coating layer facing the adjacent positive electrode sheet. The negative electrode sheet inside is coated on both sides. There are 9 positive electrode sheets, all of which are coated on both sides.
[0138] Description: The bare cell is composed of a positive electrode sheet-a first separator-an electrothermal layer-a second separator-a negative electrode sheet as a basic unit, and the first separator coated with an electrothermal layer and the second separator are stacked in a Z-shaped manner.
[0139] 5) Ear welding:
[0140] The positive electrode tabs of the bare cell are folded and welded together, and then the aluminum tabs (first tabs) are welded on; the negative electrode tabs are folded and welded together, and then the nickel tabs (second tabs) are welded on; first, T-shaped copper foils (5 μm thick) with a width of 4.0 mm and a side length of 20.0 mm are respectively attached to the two silver electrodes of the electrothermal layer, and then the copper foils are respectively welded to the other two nickel tabs (third tabs and fourth tabs), as shown in the schematic diagram. Fig. 9 .
[0141] 6) Perform conventional subsequent packaging on the bare battery cell with the tabs welded to it:
[0142] The details are as follows:
[0143] Bagging and packaging:
[0144] Select an aluminum-plastic film bag with openings on the top and bottom sides and the right side, and the size of the aluminum-plastic film bag is larger than the bare battery cell; put the bare battery cell with the electrode tabs welded obtained in step 5) into the aluminum-plastic film bag, at this time, the ends of the first electrode tab and the third electrode tab are exposed at the top edge of the aluminum-plastic film bag, and the ends of the second electrode tab and the fourth electrode tab are exposed at the bottom edge of the aluminum-plastic film bag. The top edge and the side edge without airbags of the aluminum-plastic film bag are packaged.
[0145] Vacuum baking: Bake the bagged cells in a vacuum environment at 85°C for 6 hours;
[0146] Liquid injection: vacuum inject 3.0mL of electrolyte into the baked battery cell and let it stand for 2h;
[0147] Degassing and side sealing:
[0148] The battery cell after liquid injection is degassed, and then the other side of the aluminum-plastic film bag with the air bag is packaged.
[0149] Standing: Let the packaged soft-pack battery stand at 70°C for 6 hours.
[0150] Cut the air pocket: Cut the air pocket of the battery and seal the side.
[0151] Note: The air bag is a piece extended from the aluminum-plastic film and is finally cut off; the size of the aluminum-plastic film is larger than the final battery cell.
[0152] The internally heated battery prepared in this way does not require a clamp because the internal contact is good.
[0153] Its schematic diagram is as follows Fig.10 .
[0154] Embodiment 3: A wound internal heating battery, comprising the following steps:
[0155] 1) The preparation of the electrothermal layer is the same as step 1) of Example 1;
[0156] 2) Diaphragm cutting:
[0157] The second diaphragm and the first diaphragm provided with the electrothermal layer were cut into 94.0×1751.8 mm, respectively. That is, the first diaphragm and the second diaphragm had the same size.
[0158] 3) Pole cutting:
[0159] The positive electrode sheet is a ternary positive electrode sheet, and the positive electrode sheet is coated on both sides; the negative electrode sheet is a graphite negative electrode sheet, and the negative electrode sheet is coated on one side or on both sides.
[0160] The positive electrode sheet is cut to 89.5×1451.8mm, and the negative electrode sheet is cut to 91.0×1601.8mm.
[0161] 4) Bare battery cell assembly:
[0162] The bare cell is assembled using a winding process. The bare cell uses the positive electrode sheet-first diaphragm-electrothermal layer-second diaphragm-negative electrode sheet as a basic unit. The negative electrode sheet on the outermost layer is coated on one side with the coating layer facing the positive electrode sheet. The negative electrode sheet on the inner layer is coated on both sides, and the positive electrode sheets are all coated on both sides.
[0163] 5) Ear welding:
[0164] An aluminum pole tab (first pole tab) is welded on the positive pole tab of the bare battery cell; a nickel pole tab (second pole tab) is welded on the negative pole tab; first, a T-shaped copper foil (5 μm thick) with a width of 4.0 mm and a side length of 20.0 mm is respectively attached to the two silver electrodes of the electrothermal layer, and then the copper foil is respectively welded to the other two nickel pole tabs (third pole tab and fourth pole tab). Its structure is similar to that of Example 2.
[0165] 6) Change the injection amount of the electrolyte from "3.0 mL" to "10 mL", and the rest is the same as step 6) of Example 2.
[0166] Comparative experiment 1: Test of the electrothermal performance of the diaphragm not coated with the electrothermal layer:
[0167] Cut a piece of 2.5×4.5cm 2 The diaphragm (bare diaphragm) is not coated with an electrothermal layer, a thermocouple is attached to the back, and the two short sides of the diaphragm are respectively connected to the two poles of a DC power supply.
[0168] Connect 15, 20, 25 or 30V DC respectively and record the temperature change of the thermocouple.
[0169] The temperature recorded by the thermocouple did not change. Therefore, it can be concluded that the diaphragm not coated with the electrothermal layer is electronically insulating and has no electrothermal capability.
[0170] Comparative experiment 2: Performance test of the diaphragm not coated with the electrothermal layer:
[0171] 1) Thermal stability test:
[0172] The diaphragm without the electrothermal layer was tested by differential scanning calorimetry, with a heating rate of 3°C / min and nitrogen as the protective gas.
[0173] The recorded data is as follows Fig.11 , the closed-cell and melting peak temperatures of the separator are 159.5 and 165.5 °C, respectively.
[0174] The diaphragm without the electrothermal layer was tested in a thermostatic box at a temperature of 180°C and a holding time of 30 minutes.
[0175] The recorded data is as follows Fig.12 , the heat shrinkage rate of the diaphragm is 54.5%.
[0176] Compared with the present invention Figure 6 and Figure 7 It can be seen that the electrothermal layer improves the thermal stability of the diaphragm.
[0177] 2) Wettability test:
[0178] The contact angle meter was used to test the substrate not coated with the electrothermal layer, and the liquid medium was an electrolyte.
[0179] The recorded data is as follows Fig.13 , the static contact angle of the electrothermal layer is 39.9°.
[0180] Compared with the present invention Figure 8 It can be seen that the electrothermal layer improves the wettability of the diaphragm.
[0181] In summary, the electrothermal layer has fast, uniform and adjustable electrothermal capability. After integrating the electrothermal layer into the battery cell, internal heating of the battery cell can be achieved. Compared with the bare diaphragm, the introduction of the electrothermal layer can improve the thermal stability and wettability of the diaphragm, thereby improving the thermal safety and electrochemical performance of the battery.
[0182] Comparative Example 1: Change the mixture I in the dual conductive slurry from "lithium aluminum titanium phosphate, carbon nanotubes and polyvinylidene fluoride in a mass ratio of 85:10:5" to "lithium aluminum titanium phosphate and polyvinylidene fluoride in a mass ratio of 95:5", and the rest is the same as the preparation of the electrothermal layer in step 1) of Example 1.
[0183] The coated diaphragm obtained was tested according to the method described in the above Experiment 1, and the result obtained was: the coating layer had no electrothermal property.
[0184] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. An internally heated battery, comprising a bare cell, an electrolyte and a casing, characterized in that: A bare cell immersed in an electrolyte is sealed in a housing, wherein the bare cell comprises a positive electrode, a negative electrode, a separator, an electrothermal layer and a tab, wherein the separator comprises a first separator and a second separator, and the tab comprises a first tab, a second tab, a third tab and a fourth tab; The positive electrode, the first diaphragm, the electrothermal layer, the second diaphragm, and the negative electrode are arranged in sequence; the first electrode tab is electrically connected to the positive electrode, the second electrode tab is electrically connected to the negative electrode, and the third electrode tab and the fourth electrode tab are electrically connected to both ends of the electrothermal layer, respectively.
2. The internally heated battery according to claim 1, characterized in that: The bare cell assembly is performed by lamination or winding.
3. The internally heated battery according to claim 1 or 2, characterized in that: The electrothermal layer has electronic conductivity and ionic conductivity.
4. The internally heated battery according to claim 3, characterized in that: The electrothermal layer consists of an electrothermal body layer and a conductive electrode; conductive electrodes are respectively arranged at two ends of the electrothermal layer, and the third pole ear and the fourth pole ear are respectively connected to corresponding conductive electrodes.
5. The method for preparing an internal heating battery according to any one of claims 1 to 4, characterized in that The following steps are involved: 1) Preparation of electrothermal layer: The electrothermal layer is composed of an electrothermal body layer and a conductive electrode; The electrothermal material slurry is applied to the entire surface of the first diaphragm facing the second diaphragm, and then dried to form an electrothermal body layer with a thickness of 1 to 10 μm; The electrothermal material is composed of an ionic conductive agent, an electronic conductive agent I and a binder I with mass contents of 84-86%, 9-11% and 4.5-5.5% respectively; The conductive electrode material slurry is coated on the left and right ends of the electrothermal body layer respectively, and then dried to form two strip-shaped conductive electrodes located on the electrothermal body layer; The conductive electrode material is composed of an electronic conductive agent II and a binder II with mass contents of 89-91% and 9-11% respectively; 2) Cutting a second diaphragm having a surface area consistent with that of the first diaphragm; 3) Pole cutting: The surface area of the positive electrode sheet is smaller than that of the negative electrode sheet, and the surface area of the negative electrode sheet is smaller than that of the first separator; 4) Bare battery cell assembly: The bare cell assembly adopts a lamination or winding process, and the basic unit of the bare cell is a positive electrode sheet-a first diaphragm-an electrothermal layer-a second diaphragm-a negative electrode sheet; 5) Ear welding: The positive electrode sheet is welded with the first pole ear, the negative electrode sheet is welded with the second pole ear, and the third pole ear and the fourth pole ear are respectively connected to the conductive electrode of the electric heating layer; and a bare battery cell with the pole ears welded thereon is obtained; 6) The bare battery cell with the tabs welded thereto is subsequently packaged to obtain an internally heated battery.
6. The method for preparing an internal heating battery according to claim 5, characterized in that: The ion conductive agent is lithium aluminum titanium phosphate, the electronic conductive agent I is carbon nanotubes, and the binder I is polyvinylidene fluoride; The electronic conductive agent II is silver nanowire, and the binder II is polyvinylidene fluoride.
7. The method for preparing an internal heating battery according to claim 6, characterized in that: The electrothermal material is composed of an ionic conductive agent, an electronic conductive agent I and a binder I in a mass ratio of 85:10:5; The conductive electrode material is composed of an electronic conductive agent II and a binder II in a mass ratio of 90:
10.
8. The method for preparing an internal heating battery according to any one of claims 5 to 7, characterized in that: Subsequent packaging processing includes bagging and packaging, vacuum baking, liquid injection, degassing and packaging, and standing.
9. The method for preparing an internal heating battery according to any one of claims 5 to 8, characterized in that: The first separator and the second separator are both polyolefin porous films.
10. The method for preparing an internal heating battery according to any one of claims 5 to 8, characterized in that: The electrothermal material slurry is composed of the electrothermal material with a mass concentration of 30-35% and a solvent as the balance; The conductive electrode material slurry consists of the conductive electrode material with a mass concentration of 4-6% and a solvent as the balance.