Electrolyte diaphragm for copper ion battery as well as preparation method and application of electrolyte diaphragm

By using an electrolyte separator composed of zeolite, copper salt and binder in copper-iodine batteries, the problem of multi-iodine shuttle effect is solved, the circulation efficiency and stability of copper-iodine batteries are improved, and high capacity and high stability are achieved battery performance.

CN118983616AActive Publication Date: 2024-11-19SUZHOU UNIV

Patent Information

Application Number
CN202410954456.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-19
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Due to the insoluble CuI and the shuttle properties of I-ions in copper-iodine batteries, the Coulomb efficiency and capacity decay are difficult to effectively solve the shuttle effect of multiple iodides.

Method used

Using an electrolyte membrane including zeolite, copper salt and binder, the natural pore structure and negative charge state of zeolite prevent the shuttle of iodine negative ions, the copper salt increases the concentration and transmission speed of copper ions in the membrane, and the binder connects zeolite particles to enhance Ion transport capability.

Benefits of technology

It significantly improves the circulation efficiency and stability of copper-iodine batteries, prevents the shuttle effect of iodine negative ions, and improves the coulomb efficiency and long-term service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983616A_ABST
    Figure CN118983616A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolyte diaphragm for a copper ion battery and a preparation method and application of the electrolyte diaphragm, the electrolyte diaphragm comprises zeolite, copper salt and a binder, and the mass ratio of the zeolite to the copper salt to the binder is (1-9): (1-9): (1-9). The zeolite, the copper salt and the binder are mixed, subjected to compression molding and dried to prepare the electrolyte diaphragm for the copper ion battery, the preparation process is simple, the operation is convenient, and when the prepared electrolyte diaphragm is used for the water-based copper ion battery, the electrolyte diaphragm has good ion transmission performance, can prevent the shuttle effect of iodine anions, and can improve the service life of the water-based copper ion battery. And the cycle efficiency and the stability of the copper-iodine battery are greatly improved. By utilizing the electrolyte diaphragm disclosed by the invention, a water-based copper-iodine battery with high capacity and high stability can be constructed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of copper ion battery materials, and in particular to an electrolyte diaphragm for copper ion batteries and a preparation method and application thereof. Background Art

[0002] Aqueous ion batteries have the characteristics of low cost, high safety and low environmental impact, and have received widespread attention in recent years. Among the many aqueous ion batteries, aqueous copper ion batteries have become a key research direction. First of all, the abundance and availability of copper resources give copper ion batteries a natural advantage in material sources. Secondly, the high specific capacity of copper ion batteries (837.5mAh / g) means that they can store a lot of electrical energy, which is especially important for application scenarios that require large-capacity storage. More importantly, the chemical properties of copper in aqueous solution are extremely stable, which is crucial to ensuring the long-term service life and safety of the battery.

[0003] The electrode materials used to store copper ions are mainly chalcogens. Sulfur (S) electrodes can provide an ultra-high specific capacity of 3044 mAh / g when storing copper ions (Angew.Chem.2019,131,12770). In order to cope with the shuttle effect of sulfur and its expansion problem, Wang et al. proposed a self-supporting CuS electrode (ACS Nano 2021,15,5420). In order to improve the rate performance of the CuS electrode, a Chinese patent (patent publication number: CN115028189A) discloses a method for preparing a Se-doped CuS electrode. Doping can expand the ion transmission channel and enhance the electronic conductivity of the CuS electrode. A Chinese patent (patent publication number: CN115133109A) discloses a Te positive electrode obtained by fully mixing a single Te powder with a conductive agent and a binder. These materials all achieve good electrochemical properties when paired with metallic copper.

[0004] In addition to chalcogenide electrodes, iodine (I2) electrodes are also used in aqueous battery systems such as zinc-iodine (Zn / / I2) batteries due to their high capacity and low cost. In Zn / / I2 batteries, Zn is used as the negative electrode due to its low potential, while I2 is used as the positive electrode due to its high potential. Similarly, copper-iodine (Cu / / I2) batteries can also be designed. In Cu / / I2 batteries, due to the low potential of Cu 2+ / Cu standard potential 0.34V compared to I2 / I - The standard potential of CuI is lower than 0.54V. This reaction seems to be unable to proceed spontaneously, but due to the formation of insoluble products of CuI, Cu 2+ Can oxidize I - ions, the reaction that occurs at this time is 2Cu 2+ +4I -→2CuI+I2, the standard potential can reach 0.86V. This reaction is the iodine titration method commonly used in analytical chemistry. However, due to the poor solubility of CuI and I - The shuttling nature of ions (i.e., the generated polyiodides will shuttle to the negative electrode for direct reduction) causes problems of low coulombic efficiency and capacity decay, making the iodine titration reaction difficult to use for building batteries. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an electrolyte membrane for copper ion batteries and a preparation method and application thereof. The preparation process is simple and the operation is convenient. When the prepared electrolyte membrane is used in an aqueous copper ion battery, the coulombic efficiency and cycle stability of the battery can be improved, and the problem of the shuttle effect of multiple iodides in aqueous copper iodine batteries can be solved.

[0006] The present invention is achieved through the following technical solutions:

[0007] A first aspect of the present invention provides an electrolyte membrane for a copper ion battery, wherein the electrolyte membrane comprises zeolite, a copper salt and a binder, wherein the mass ratio of the zeolite, the copper salt and the binder is (1-9):(1-9):(1-9).

[0008] In the electrolyte membrane provided by the present invention, the natural pore structure of zeolite helps to improve the transmission speed of ions, and its limited pore size and the charged state of negative charge can effectively prevent the passage of larger iodine anions, thereby inhibiting the shuttle effect of iodine anions. In addition, zeolite powder has good chemical stability in aqueous electrolytes, which helps to enhance the long-term cycle stability of the battery. The addition of copper salt helps to increase the copper ion concentration inside the membrane, thereby enhancing the ion transfer speed of the membrane. The addition of a binder helps to connect the zeolite powder particles, thereby reducing the transmission distance of copper ions and improving the ion transmission capacity of the electrolyte membrane.

[0009] Furthermore, the chemical formula of the zeolite is A m B q O 2q nH2O, wherein A is selected from one or more of calcium (Ca), sodium (Na), potassium (K), barium (Ba) and strontium (Sr), and B is aluminum (Al) and silicon (Si).

[0010] Furthermore, in the chemical formula of the zeolite, q is the valence of the cation, q is 1-2, m is the number of cations, m is 1-5, preferably 2-5, and n is the number of water molecules, n is 1-20, preferably 4.5-14.

[0011] Furthermore, the structural formula of the zeolite is A m [(AlO2) x (SiO2)y ]·n(H2O), wherein x is the number of Al atoms, x is 1 to 5, preferably 2 to 5, y is the number of Si atoms, y is 1 to 15, preferably 2 to 13, y / x (Si / Al ratio) is 1 to 5, preferably 1 to 2.6, and x+y is the number of tetrahedrons in the unit cell.

[0012] Furthermore, the mass ratio of the zeolite, the copper salt and the binder is preferably (2-5):(2-5):(1-3), and more preferably (3-5):(3-5):(1-3).

[0013] Furthermore, the copper salt is selected from one or more of copper sulfate, copper chloride, copper bromide, copper acetate and copper trifluoromethanesulfonate.

[0014] Furthermore, the binder is selected from one or more of polytetrafluoroethylene (PTFE), polyacrylonitrile (PAN) and polypropylene (PAA).

[0015] Furthermore, the electrolyte separator has a thickness of 10 to 50 μm.

[0016] A second aspect of the present invention provides a method for preparing an electrolyte membrane for a copper ion battery, comprising the following steps:

[0017] (1) mixing zeolite, copper salt, a binder and water to obtain a mixture;

[0018] (2) The mixture obtained in step (1) is pressed into shape, and dried to obtain the electrolyte membrane.

[0019] Furthermore, in step (1), the zeolite is subjected to a vacuum activation treatment, the activation treatment temperature is 100-200° C., and the activation treatment time is 1-10 h, that is, the zeolite is placed in a vacuum at 100-200° C. and stored for 1-10 h.

[0020] In a specific embodiment, in step (1), the activated zeolite powder and copper salt powder are first ground and stirred, and then the binder powder and water are added and mixed evenly.

[0021] Furthermore, the particle size of the zeolite powder is 2 to 5 μm.

[0022] Furthermore, in step (2), the pressure of the compression molding is 1 to 10 MPa.

[0023] Furthermore, in step (2), the drying is carried out by vacuum drying.

[0024] Furthermore, in step (2), the drying temperature is 50 to 150°C.

[0025] Furthermore, in step (2), the drying time is 1 to 10 hours.

[0026] The third aspect of the present invention provides the use of the electrolyte membrane for copper ion batteries described in the first aspect in the preparation of copper ion batteries, especially copper iodine batteries.

[0027] When the electrolyte membrane of the present invention is used in an aqueous copper ion battery, it has good ion transmission performance, can prevent the shuttle effect of iodine anions, and greatly improves the cycle efficiency and stability of the copper iodine battery. The electrolyte membrane of the present invention can be used to construct an aqueous copper iodine battery with high capacity and high stability.

[0028] The present invention provides a highly reversible Cu / / I2 battery, which uses a composite electrode of iodine and carbon black to solve the reversibility problem of CuI, and uses a zeolite-based electrolyte membrane with high ion conductivity and the characteristics of inhibiting anion shuttle, thereby greatly improving the cycle efficiency and stability of the copper-iodine battery. The Cu / / I2 battery is significantly different from the Zn / / I2 battery. On the one hand, the Zn in the Zn / / I2 battery 2+ Ions are only charge carriers, and Cu in Cu / / I2 batteries 2+ The ions are not only charge carriers but also redox active centers, which can be further reduced to Cu + ions; on the other hand, in a Zn / / I2 cell, I2 oxidizes Zn to form I - Ions and Zn 2+ ions, I2 is the positive electrode; in the Cu / / I2 battery, I2 first obtains electrons and is reduced to I - ions, and then the Cu 2+ Ions are oxidized to generate I2 and Cu + ions, so I2 and Cu in the electrolyte 2+ They are all positive electrode materials.

[0029] Beneficial effects of the present invention:

[0030] The preparation process of the electrolyte membrane provided by the present invention is simple and easy to operate. When the prepared electrolyte membrane is used in an aqueous copper ion battery, the addition of zeolite and copper salt can significantly improve the ion transmission capacity of the electrolyte membrane. The natural pore structure of the zeolite is a rapid ion transmission channel. At the same time, the addition of copper salt helps to increase the copper ion concentration of the electrolyte membrane, further improve the copper ion transmission performance, and thus improve the coulomb efficiency and cycle stability of the battery. The rigid crystal framework of the zeolite carries a natural negative charge and can repel polyiodide ions with the same negative charge. At the same time, its limited pore size can prevent the passage of larger iodine anions, so the problem of the shuttle effect of polyiodides in aqueous copper-iodine batteries can be solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is an optical photograph of the electrolyte membrane of Example 1.

[0032] Figure 2 This is a charge and discharge curve of an aqueous copper-iodine battery assembled with the electrolyte membrane of Example 1 and a glass fiber membrane at 0.2 A / g.

[0033] Figure 3 This is a comparison chart of the cycle performance of an aqueous copper-iodine battery assembled with the electrolyte membrane of Example 1 and a glass fiber membrane at 1 A / g.

[0034] Figure 4 This is a cycling performance diagram of an aqueous copper-iodine battery assembled with the electrolyte membrane of Example 1 at 2.0 A / g.

[0035] Figure 5 Graph showing the ionic conductivity data of the electrolyte membranes of Examples 1 to 9. DETAILED DESCRIPTION

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0038] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0039] The test method of the electrochemical performance of the electrolyte membrane in the following embodiments is as follows:

[0040] Ionic conductivity: A pressure of 0 to 5 MPa was applied to the electrolyte membrane, and then a blocking electrode test was performed by clamping stainless steel sheets with a diameter of 16 mm and a thickness of 100 μm on both sides of the electrolyte membrane to prepare a blocking electrode. Subsequently, an electrochemical impedance spectroscopy test was performed, and the measured results were input into the formula δ=d / RA, where δ in the formula represents ionic conductivity, d is the thickness of the membrane, R is the resistance, and A is the interface area of ​​the membrane.

[0041] The electrolyte membranes in the following embodiments are assembled into aqueous copper-iodine batteries, and the assembly method is as follows:

[0042] A composite electrode prepared by uniformly mixing iodine, carbon black and a binder in a mass ratio of 8:1:1 is used as a working electrode, a pure copper sheet is used as a counter electrode, a 0.5M CuSO4 aqueous solution is used as an electrolyte, and the electrolyte membrane of the present invention is combined to assemble an aqueous copper-iodine battery.

[0043] The voltage range of the charge and discharge test of the assembled aqueous copper-iodine battery is 0.1 to 0.6V.

[0044] Example 1

[0045] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 4:5:1, and a preparation method comprises the following steps:

[0046] (1) Zeolite powder (Na2[Al2Si2O8]·4.5H2O) was activated in a vacuum at 200°C for 1 h. 640 mg of the activated zeolite powder and 800 mg of copper sulfate powder were ground and stirred in a mortar. Then, 160 mg of polytetrafluoroethylene powder and water were added and mixed evenly to obtain a paste mixture.

[0047] (2) The paste mixture obtained in step (1) is pressed under a pressure of 8 MPa into an electrolyte membrane with a thickness of 15 μm, and vacuum dried at 50° C. for 5 h to obtain an electrolyte membrane, such as Figure 1 shown.

[0048] A pressure of 3 MPa was applied to the electrolyte membrane, and the ionic conductivity of the electrolyte membrane of Example 1 was measured to be 3.1 mS / cm through a blocked electrode test.

[0049] Figure 2 The charge and discharge curve of the aqueous copper-iodine battery assembled with the electrolyte membrane and the glass fiber membrane of Example 1 at a current density of 0.2 A / g is shown in FIG. Figure 2 It can be seen that the first-cycle discharge capacity of the aqueous copper-iodine battery based on the electrolyte membrane of Example 1 is 347 mAh / g, and the first-cycle coulomb efficiency is 97%; the first-cycle discharge capacity of the aqueous copper-iodine battery based on the glass fiber membrane is 198 mAh / g, and the first-cycle coulomb efficiency is 61%.

[0050] Figure 3 The comparison chart of the cycle performance of the aqueous copper-iodine battery assembled with the electrolyte membrane and the glass fiber membrane of Example 1 at 1A / g is shown in FIG. Figure 3 It can be seen that the 100-cycle capacity retention rate of the aqueous copper-iodine battery based on the electrolyte membrane of Example 1 is as high as 92%, while the capacity retention rate of the aqueous copper-iodine battery based on the glass fiber membrane after 100 cycles is only 12%.

[0051] Figure 4 The cycle performance diagram of the aqueous copper-iodine battery assembled with the electrolyte membrane of Example 1 at 2.0A / g is shown in FIG. Figure 4 It can be seen that the copper-iodine battery still maintains 95.7% of its initial capacity after 600 cycles.

[0052] Example 2

[0053] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 3:3:1, and the preparation method is basically the same as that of Example 1.

[0054] Example 3

[0055] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 3:4:2, and the preparation method is basically the same as that of Example 1.

[0056] Example 4

[0057] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 3:5:3, and the preparation method is basically the same as that of Example 1.

[0058] Example 5

[0059] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 4:3:2, and the preparation method is basically the same as that of Example 1.

[0060] Example 6

[0061] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 4:4:3, and the preparation method is basically the same as that of Example 1.

[0062] Example 7

[0063] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 5:4:1, and the preparation method is basically the same as that of Example 1.

[0064] Example 8

[0065] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 5:5:2, and the preparation method is basically the same as that of Example 1.

[0066] Example 9

[0067] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper sulfate and polytetrafluoroethylene is 5:5:3, and the preparation method is basically the same as that of Example 1.

[0068] Figure 5 Graph showing the ionic conductivity data of the electrolyte membranes of Examples 1 to 9.

[0069] Example 10

[0070] An electrolyte membrane comprises Na2[Al2Si2O8]·4.5H2O, copper acetate and polyacrylic acid, wherein the mass ratio of Na2[Al2Si2O8]·4.5H2O, copper acetate and polyacrylic acid is 5:4:1, and the preparation method comprises the following steps:

[0071] (1) Zeolite powder (Na2[Al2Si2O8]·4.5H2O) was activated in a vacuum at 100°C for 10 h, 800 mg of the activated zeolite powder and 640 mg of copper acetate powder were ground and stirred in a mortar, and then 160 mg of polyacrylic acid powder and water were added and mixed evenly to obtain a paste mixture.

[0072] (2) The paste mixture obtained in step (1) is pressed into an electrolyte membrane with a thickness of 50 μm at a pressure of 1 MPa, and vacuum dried at 100° C. for 2 h to obtain an electrolyte membrane.

[0073] A pressure of 3 MPa was applied to the electrolyte membrane, and the ionic conductivity of the electrolyte membrane of Example 10 was measured to be 3.7 mS / cm by blocking the electrode test. The aqueous copper-iodine battery assembled with the electrolyte membrane of Example 10 had a first-cycle discharge capacity of 345 mAh / g and a first-cycle coulomb efficiency of 96% at a current density of 0.2 A / g; at a current density of 1 A / g, the capacity retention rate after 100 cycles was as high as 91%.

[0074] Embodiment 11

[0075] An electrolyte membrane comprising NaCa2[Al5Si 13 O 36 ]·14H2O, copper bromide and polyacrylonitrile, among which NaCa2[Al5Si 13 O 36 ]·The mass ratio of 14H2O, copper bromide and polyacrylonitrile is 5:3:2, and the preparation method comprises the following steps:

[0076] (1) Zeolite powder (NaCa2[Al5Si 13 O 36 ]·14H2O) was placed in a vacuum at 150°C for activation treatment for 5 hours, 800 mg of the activated zeolite powder and 480 mg of copper bromide powder were placed in a mortar and ground and stirred, and then 320 mg of polyacrylonitrile powder and water were added and mixed evenly to obtain a paste mixture.

[0077] (2) The paste mixture obtained in step (1) was pressed into an electrolyte membrane with a thickness of 35 μm at a pressure of 5 MPa, and vacuum dried at 80° C. for 3 h to obtain an electrolyte membrane.

[0078] A pressure of 3 MPa was applied to the electrolyte membrane, and the ionic conductivity of the electrolyte membrane of Example 11 was measured to be 4.9 mS / cm by blocking the electrode test. The aqueous copper-iodine battery assembled with the electrolyte membrane of Example 11 had a first-cycle discharge capacity of 355 mAh / g and a first-cycle coulomb efficiency of 97% at a current density of 0.2 A / g; at a current density of 1 A / g, the capacity retention rate after 100 cycles was as high as 91%.

[0079] Example 12

[0080] An electrolyte membrane comprising NaCa2[Al5Si 13 O 36 ]·14H2O, copper trifluoromethanesulfonate and polytetrafluoroethylene, among which NaCa2[Al5Si 13 O 36 The mass ratio of 14H2O, copper trifluoromethanesulfonate and polytetrafluoroethylene is 4:5:1, and the preparation method comprises the following steps:

[0081] (1) Zeolite powder (NaCa2[Al5Si 13 O 36 ]·14H2O) was placed in a vacuum at 180°C for activation treatment for 2 hours, 640 mg of the activated zeolite powder and 800 mg of copper trifluoromethanesulfonate powder were placed in a mortar and ground and stirred, and then 160 mg of polytetrafluoroethylene powder and water were added and mixed evenly to obtain a paste mixture.

[0082] (2) The paste mixture obtained in step (1) is pressed into an electrolyte membrane with a thickness of 10 μm at a pressure of 10 MPa, and vacuum dried at 150° C. for 1 h to obtain an electrolyte membrane.

[0083] A pressure of 3 MPa was applied to the electrolyte membrane, and the ionic conductivity of the electrolyte membrane of Example 12 was measured to be 3.2 mS / cm by blocking the electrode test. The aqueous copper-iodine battery assembled with the electrolyte membrane of Example 12 had a first-cycle discharge capacity of 350 mAh / g and a first-cycle coulomb efficiency of 93% at a current density of 0.2 A / g; at a current density of 1 A / g, the capacity retention rate after 100 cycles was as high as 90%.

[0084] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. An electrolyte membrane for a copper ion battery, characterized in that: The electrolyte membrane comprises zeolite, copper salt and a binder, wherein the mass ratio of zeolite, copper salt and binder is (1-9):(1-9):(1-9).

2. The electrolyte membrane for copper ion battery according to claim 1, characterized in that: The chemical formula of the zeolite is A m B q O 2q nH2O, wherein A is selected from one or more of calcium, sodium, potassium, barium and strontium, B is aluminum and silicon, m is 1 to 5, q is 1 to 2, and n is 1 to 20.

3. The electrolyte membrane for copper ion battery according to claim 1, characterized in that: The copper salt is selected from one or more of copper sulfate, copper chloride, copper bromide, copper acetate and copper trifluoromethanesulfonate.

4. The electrolyte membrane for copper ion battery according to claim 1, characterized in that: The binder is selected from one or more of polytetrafluoroethylene, polyacrylonitrile and polyacrylic acid.

5. The electrolyte membrane for copper ion battery according to claim 1, characterized in that: The electrolyte separator has a thickness of 10 to 50 μm.

6. The method for preparing an electrolyte membrane for a copper ion battery according to claim 1, characterized in that: The following steps are involved: (1) mixing zeolite, copper salt, a binder and water to obtain a mixture; (2) The mixture obtained in step (1) is pressed into shape, and dried to obtain the electrolyte membrane.

7. The preparation method according to claim 6, characterized in that: In step (1), the zeolite is subjected to vacuum activation treatment, the activation treatment temperature is 100 to 200° C., and the activation treatment time is 1 to 10 hours.

8. The preparation method according to claim 6, characterized in that: In step (2), the pressure of the compression molding is 1 to 10 MPa.

9. The preparation method according to claim 6, characterized in that: In step (2), the drying temperature is 50 to 150°C.

10. Use of the electrolyte membrane for copper ion batteries according to any one of claims 1 to 5 in the preparation of copper ion batteries.

Citation Information

Patent Citations

  • Copper ion battery positive electrode material and preparation method thereof

    CN115028189A

  • Water-based copper ion battery

    CN115133109A

  • Zeolite-based ion exchange coating for long-life zinc-iodine battery

    CN114552029A

  • Iodine secondary battery of adsorbent positive electrode material

    CN114725533A

Cited By

  • Water-based miniature copper battery and preparation method thereof