Method for preparing bromine and chlorine mixed all-inorganic perovskite thin film in high-humidity air environment

By using a two-step spin coating process and additives in a high-humidity air environment, a high-performance zero-dimensional-three-dimensional biphasic perovskite film was prepared, which solved the problem of complexity and cost of preparing perovskite films in the prior art. , achieving film preparation and performance improvement suitable for commercial production.

CN118984633APending Publication Date: 2024-11-19ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411056959.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to prepare high-performance perovskite films in high humidity air environments, resulting in increased manufacturing complexity and cost, and lack of methods suitable for large-scale commercial production.

Method used

The mixed bromochlorochloro-all-inorganic perovskite film was prepared in a high humidity air environment using a two-step spin coating process. The film was limited by adding tetraphenylphosphorus halide and Tween 20 to the spin coating solution in the first and second steps. Phase growth and assisted ion diffusion to generate biphasic perovskite components through thermal annealing to regulate emission wavelength.

Benefits of technology

It realizes the growth of zero-dimensional-3D biphasic perovskite films with high surface coverage and high optical quality in high humidity environment, reducing the impact of water and oxygen on the perovskite generation process, and is suitable for light emission of light emitting diode devices. medium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984633A_ABST
    Figure CN118984633A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of semiconductor materials and photoelectricity, and particularly relates to a method for preparing a bromine and chlorine mixed all-inorganic perovskite thin film in a high-humidity air environment, the preparation is carried out by using a two-step spin coating process in the high-humidity air environment, the prepared perovskite thin film has a zero-dimensional-three-dimensional double-phase structure, the chemical formula is Cs4Pb (Br1-xClx) 6-CsPb (Br1-xClx) 3, wherein 0 lt; xlt; 1. According to the invention, due to the existence of the zero-dimensional perovskite, the defects in a three-dimensional perovskite crystallization process in a high-humidity air environment are inhibited, so that the material has relatively high photoluminescence performance; due to the fact that the two-step spin-coating process is used and low precursor concentration is adopted, the film layer has low thickness and keeps high surface coverage rate, and therefore the film layer is very suitable for being used as a light-emitting layer of a light-emitting diode and is applied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor materials and optoelectronic technology, and specifically relates to a method for preparing a mixed bromine-chlorine all-inorganic perovskite film in a high-humidity air environment. Background Art

[0002] Metal halide perovskites have broad application prospects in the field of optoelectronic devices due to their low raw material cost, excellent optoelectronic properties, easy spectrum adjustment, and simple processing technology. Since the first report of room temperature electroluminescent devices, the performance of their light-emitting diodes has been in a state of rapid development. The external quantum efficiency in the near-infrared, red, and green bands has approached the commercial standard, making them a promising candidate for future high-quality lighting and high-end display applications. However, almost all high-performance perovskite light-emitting diodes (PeLEDs) need to be prepared in an inert or dry atmosphere to reduce the adverse effects of humidity and air on perovskite crystallization, which inevitably increases manufacturing complexity and cost. Therefore, developing processing strategies in ambient atmospheres will help reduce the manufacturing cost of PeLEDs and promote their industrial application.

[0003] At present, the academic community mainly uses two methods to prepare perovskite films suitable for light-emitting diodes in a non-inert environment. The first method is to strictly control the water and oxygen content in the environment during the nucleation and crystallization of perovskite, such as using inert gases such as nitrogen to blow to isolate water and oxygen during the spin coating of the perovskite precursor, or directly controlling the water and oxygen in the environment at a low level. At present, the external quantum efficiency of light-emitting diode devices based on this method has exceeded 15%. However, this method requires strict control of environmental humidity and temperature, which is not conducive to low-cost industrial production. Another method is to select a suitable substrate material to reduce water and oxygen adsorption to control the crystallization dynamics. For example, using a self-assembled monolayer as the hole transport layer of the device and a substrate for the perovskite precursor solution in a non-inert environment, a quasi-two-dimensional cesium-based lead bromide (CsPbBr3) film can be prepared in an environment with a humidity of up to 60%. At present, the brightness of the light-emitting diode device based on this method exceeds 20,000 cd m -2 . However, the self-assembled monolayer used in this method requires a complex chemical synthesis process and can only be produced in small batches on a laboratory scale. In addition, the effect of the monolayer on device performance needs to be further improved. Therefore, it is necessary to develop a method that is compatible with large-scale commercial transport materials and can effectively regulate the effect of water and oxygen on the crystallization process of perovskite.

[0004] The two-step spin coating method deposits the two main raw materials for forming perovskite on the substrate in sequence and evenly, and forms perovskite through interface ion diffusion during the subsequent heating and annealing process. Since the chemical reaction mainly occurs at the interface and the upper precursor film is far away from the interface, this method has a natural ability to isolate water and oxygen compared to the one-step spin coating method. At present, this method has been used to prepare thick perovskite films in non-inert environments. However, due to self-absorption, thick films are generally only suitable for solar cell devices; and the optimal film thickness of light-emitting diodes is generally only a fraction of the thickness of solar cells. At present, there are no reports at home and abroad on the use of a two-step spin coating process in a high humidity air environment to prepare perovskite films suitable for light-emitting diode devices. Summary of the invention

[0005] The purpose of the present invention is to overcome the above problems existing in the conventional technology and provide a method for preparing a mixed bromine-chlorine all-inorganic perovskite film in a high humidity air environment.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] The present invention provides a method for preparing a mixed bromine-chlorine all-inorganic perovskite film, which is carried out using a two-step spin coating process in a high-humidity air environment. The prepared perovskite film has a zero-dimensional-three-dimensional dual-phase structure, and the chemical formula is Cs4Pb(Br 1- x Cl x )6-CsPb(Br 1-x Cl x )3, where 0 <x<1。

[0008] Furthermore, tetraphenylphosphonium halide and Tween 20 are added to the spin coating solutions in the first and second steps to restrict the phase growth in the film.

[0009] Furthermore, the spin-coated film is subjected to thermal annealing in an air environment to assist ion diffusion, and a dual-phase perovskite component is generated under the synergistic effect of tetraphenylphosphine halide and Tween 20.

[0010] Furthermore, the bandgap of the film can be adjusted by adjusting the chloride ion content in the two-step spin coating solution to control the emission wavelength from green (x=0) to deep blue (x>0.5).

[0011] Furthermore, the method specifically comprises the following steps:

[0012] 1) PbX2, tetraphenylphosphorus halide and Tween 20 are dissolved in DMF in a certain ratio, and heated and stirred in an air environment until all dissolved to obtain a solution A; in an air environment, the solution A is distributed on the surface of the substrate A by a spin coating method to obtain a substrate B;

[0013] 2) dissolving CsX, tetraphenylphosphorus halide and Tween 20 in a mixed solvent of water and isopropanol in a certain proportion to obtain a solution B, wherein X in CsX is bromine, chlorine or a mixture thereof, and the halogen in tetraphenylphosphorus halide is bromine, chlorine or a combination thereof; distributing the solution B on the surface of the substrate B by spin coating in a high humidity air environment;

[0014] 3) The obtained PbX2 / CsX double-layer film is subjected to thermal annealing in an air environment to assist ions to diffuse across the PbX2 / CsX interface and react to form a dual-phase perovskite; the annealing temperature is not higher than 150°C, and the annealing temperature and annealing time are regulated according to the thickness of the PbX2 and CsX layers until the optical, electrical and surface properties of the film are optimal.

[0015] Furthermore, in step 1), the PbX2, tetraphenylphosphorus halide and Tween 20 are dissolved in DMF in a mass ratio of 25:0.1 to 25:0.1 to 25.

[0016] Furthermore, in step 1), the substrate A is any one of a plastic film, a metal sheet, and a glass sheet.

[0017] Furthermore, in step 2), the CsX, tetraphenylphosphonium halide, and Tween 20 are dissolved in a mixed solvent of water and isopropanol in a mass ratio of 8:0.1 to 8:0.1 to 8; the volume ratio of water to isopropanol is less than 1, and the volumes of isopropanol and water are adjusted according to the mass of CsX and the chloride ion content until CsX can just be dissolved.

[0018] Furthermore, in step 2), the high humidity air environment refers to an air environment with a relative humidity of 40 to 70% rh.

[0019] The present invention also provides a mixed bromine-chlorine all-inorganic perovskite film for use in the preparation of light-emitting diodes, Cs4Pb(Br 1-x Cl x )6-CsPb(Br 1-x Cl x )3 is used as the light-emitting medium of the light-emitting diode, and a transparent bottom electrode / hole or electron transport layer / perovskite light-emitting layer / electron or transport layer / interface modification layer / counter electrode structure is adopted.

[0020] The beneficial effects of the present invention are:

[0021] The present invention provides a method for preparing a mixed bromine-chlorine all-inorganic perovskite film. The prepared film has a zero-dimensional and three-dimensional dual-phase structure, and is grown using a two-step continuous deposition method to produce a film with high surface coverage and high optical quality. Since the chemical reaction at the interface isolates water and oxygen, it is beneficial to eliminate their influence on the perovskite formation process; tetraphenylphosphorus halide and Tween 20 change the reaction path of PbX2 and CsX to generate a zero-dimensional and three-dimensional dual-phase structure, which is beneficial to the defect passivation and environmental stability of the three-dimensional perovskite; in addition, the thickness of the generated perovskite film is controllable, so it is very suitable for the light-emitting medium of the light-emitting diode device.

[0022] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0024] Figure 1 Schematic diagram of a two-step continuous deposition process;

[0025] Figure 2 This is the spectrum of the perovskite film of Example 1;

[0026] Among them, (a) is the absorption spectrum of the perovskite film with and without additives, and (b) is the photoluminescence spectrum of the perovskite film with and without additives;

[0027] Figure 3 X-ray diffraction diagrams of the perovskite film with and without additives in Example 1;

[0028] Figure 4 is a scanning electron microscope image of Example 1;

[0029] Among them, (a) and (b) are scanning electron micrographs of PbBr2 with and without additives, respectively, and (c) and (d) are scanning electron micrographs of perovskite films with and without additives, respectively;

[0030] Figure 5 is a structural diagram of a light emitting diode device in Embodiment 1-4;

[0031] Among them, ITO is the abbreviation of indium tin oxide, which acts as a transparent conductive electrode, PEODT:PSS is the abbreviation of poly[3,4-ethylenedioxythiophene]:poly(4-styrenesulfonic acid), which acts as a hole transport / electron blocking layer, Perovskite is a perovskite, and its specific composition is cesium lead bromine chlorine all-inorganic perovskite with different chlorine contents, which acts as a light-emitting layer; TPBi is the abbreviation of triphenylbenzothiophene, which acts as an electron transport / hole blocking layer; LiF is the molecular formula of lithium fluoride, which acts as an electrode modification layer, and Al is the chemical formula of aluminum, which acts as a counter electrode;

[0032] Figure 6 1 is an energy level diagram of the light emitting diode device in Example 1 and the transport layer except the perovskite layer in Examples 2-3;

[0033] Figure 7 is the spectrum of the light emitting diode device in Example 1;

[0034] Among them, (a) is the external quantum efficiency-current density diagram, (b) left and (b) right are the current density-voltage diagram and brightness-voltage diagram, respectively, and (c) is the normalized electroluminescence spectrum at maximum brightness;

[0035] Figure 8 is the spectrum of the light emitting diode device in Example 2;

[0036] Among them, (a) is the external quantum efficiency-current density diagram, (b) left and (b) right are the current density-voltage diagram and brightness-voltage diagram, respectively, and (c) is the normalized electroluminescence spectrum at maximum brightness;

[0037] Fig. 9 is the spectrum of the light emitting diode device in Example 3;

[0038] Among them, (a) is the external quantum efficiency-current density diagram, (b) left and (b) right are the current density-voltage diagram and brightness-voltage diagram, respectively, and (c) is the normalized electroluminescence spectrum at maximum brightness;

[0039] Fig.10 is the spectrum of the light emitting diode device in Example 4;

[0040] Among them, (a) is the external quantum efficiency-current density diagram, (b) left and (b) right are the current density-voltage diagram and brightness-voltage diagram, respectively, and (c) is the normalized electroluminescence spectrum at maximum brightness. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] The present invention provides a method for preparing a mixed bromine-chlorine all-inorganic perovskite film, which is carried out using a two-step spin coating process in a high-humidity air environment. The prepared perovskite film has a zero-dimensional-three-dimensional dual-phase structure, and the chemical formula is Cs4Pb(Br 1- x Cl x )6-CsPb(Br 1-x Cl x )3, where 0 <x<1。

[0043] The specific steps include:

[0044] 1) PbX2 (X is bromine, chlorine or a mixture thereof) precursor film:

[0045] PbX2, tetraphenylphosphorus halide (halogen is bromine, chlorine or a combination thereof) and Tween 20 are dissolved in DMF in a mass ratio of 25:0.1-25:0.1-25, and heated and stirred in an air environment until all dissolved. Subsequently, the solution is distributed on a target substrate by spin coating in an air environment; the thickness of the precursor film can be controlled by the mass of PbX2 and (or) the spin coating speed.

[0046] 2) CsX (X is bromine, chlorine or a mixture thereof) precursor film:

[0047] CsX, tetraphenylphosphorus halide (halogen is bromine, chlorine or a combination thereof) and Tween 20 are dissolved in a mixed solvent of isopropanol and water in a volume ratio of <1 in a mass ratio of 8:0.1-8:0.1-8, and the molar ratio of CsX to PbX2 is not less than the sum of the Cs / Pb ratios in the following chemical reaction formula:

[0048] CsX+PbX2==CsPbX3

[0049] 4CsX+PbX2==Cs4PbX6

[0050] The volumes of isopropanol and water are adjusted according to the mass of CsX and the chloride ion content until CsX can be just dissolved; then, the solution is distributed on the PbX2 substrate using a spin coating method in an air environment with a relative humidity of 40 to 70% rh.

[0051] 3) Dual-phase perovskite film:

[0052] The PbX2 / CsX double-layer film is placed in an air environment and thermal annealing is used to assist ions to diffuse across the PbX2 / CsX interface and react to form perovskite. The annealing temperature and annealing time are regulated according to the thickness of the PbX2 and CsX layers until the optical, electrical and surface properties of the film are optimized.

[0053] The relevant specific embodiments of the present invention are as follows:

[0054] Example 1

[0055] A light-emitting diode device with a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite as an active layer, specifically, preparing a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite film with a chlorine content of 0%. In this embodiment, the chlorine content is 0%, that is, the molecular formula Cs4Pb(Br 1-x Cl x )6-CsPb(Br 1-x Cl x )3, x=0. The complete device preparation process is as follows: first, on the ITO surface after ultrasonic cleaning with deionized water, acetone, and anhydrous ethanol and plasma treatment, a PEDOT:PSS film is prepared in an open air environment by spin coating, and the film preparation is completed by annealing (annealing temperature 150°C, annealing time 10 minutes); secondly, on its surface, a PbBr2 film is prepared in an open air environment by spin coating, and the film preparation is completed by annealing (annealing temperature 70°C, annealing time 10 minutes); then, on the surface of the PbBr2 film, a CsBr film is prepared in an open air environment by spin coating, and the perovskite film is prepared by annealing (annealing temperature 130°C, annealing time 10 minutes); then, the perovskite film is transferred to a high vacuum evaporation chamber, and TPBi, LiF and Al of the required thickness are prepared in turn by thermal evaporation. The effective area of ​​the light-emitting device is determined by the intersection area of ​​the Al electrode and the ITO. Finally, the light-emitting device is placed on the top of the integrating sphere, and a source meter is used to apply voltage to both ends of the device and inject current. A spectrometer is used to collect the number of photons after diffuse reflection by the integrating sphere, and the changes in current and photon number with voltage are recorded. Based on the assumption that the light-emitting device is a Lambertian body, parameters such as external quantum efficiency, brightness, luminescence peak, CIE and current efficiency that characterize the performance of the device are obtained.

[0056] The preparation process of perovskite thin film is as follows Figure 1 As shown; the absorption spectra of the grown film and the control film without additive modification are shown Figure 2 (a) shows; the photoluminescence spectra of the grown film and the control film without additive modification are shown in Figure 2 (b) shows; X-ray spectra of the grown film and the control film without additive modification are shown in Figure 3As shown; the scanning electron microscopy spectra of the grown film and the control film without additive modification are shown Figure 4 As shown; the device structure of the light emitting diode is as follows Figure 5 The corresponding energy level structure is shown in Figure 6 As shown; the performance of the light-emitting diode device based on the grown film and the control film without additive modification is shown Figure 7 shown.

[0057] Example 2

[0058] A light-emitting diode device with a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite as an active layer, specifically, a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite film with a chlorine content of 20%. In this embodiment, the chlorine content of CsX is 20%. The complete device preparation process is as follows: first, on the ITO surface that has been ultrasonically cleaned with deionized water, acetone, and anhydrous ethanol and plasma-treated, a PEDOT:PSS film is prepared in an open air environment by a spin coating process, and the film preparation is completed by an annealing process (annealing temperature 150°C, annealing time 10 minutes); secondly, on its surface, a PbBr2 film is prepared in an open air environment by a spin coating process, and the film preparation is completed by an annealing process (annealing temperature 70°C, annealing time 10 minutes); then, on the surface of the PbBr2 film, an 80% CsBr+20% CsCl film is prepared in an open air environment by a spin coating process, and the perovskite film is prepared by an annealing process (annealing temperature 130°C, annealing time 10 minutes); then, the perovskite film is transferred to a high vacuum evaporation chamber, and TPBi, LiF and Al of the required thickness are prepared in turn by thermal evaporation, and the effective area of ​​the light-emitting device is determined by the area of ​​the Al electrode and the intersection area of ​​the ITO. Finally, the light-emitting device is placed on the top of the integrating sphere, and a source meter is used to apply voltage to both ends of the device and inject current. A spectrometer is used to collect the number of photons after diffuse reflection by the integrating sphere, and the changes in current and photon number with voltage are recorded. Based on the assumption that the light-emitting device is a Lambertian body, parameters such as external quantum efficiency, brightness, luminescence peak, CIE and current efficiency that characterize the performance of the device are obtained.

[0059] The preparation process of perovskite thin film is as follows Figure 1 As shown; the device structure of the light emitting diode is as follows Figure 5 As shown; the corresponding energy level structure except the light-emitting layer is as follows Figure 6 As shown; the performance of the light-emitting diode device based on the grown thin film is shown Figure 8 shown.

[0060] Example 3

[0061] A light-emitting diode device with a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite as an active layer, specifically, a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite film with a chlorine content of 60%. In this embodiment, the chlorine content of CsX is 60%. The complete device preparation process is as follows: first, on the ITO surface that has been ultrasonically cleaned with deionized water, acetone, and anhydrous ethanol and plasma-treated, a PEDOT:PSS film is prepared in an open air environment by a spin coating process, and the film preparation is completed by an annealing process (annealing temperature 150°C, annealing time 10 minutes); secondly, on its surface, a PbBr2 film is prepared in an open air environment by a spin coating process, and the film preparation is completed by an annealing process (annealing temperature 70°C, annealing time 10 minutes); then, on the surface of the PbBr2 film, a 40% CsBr+60% CsCl film is prepared in an open air environment by a spin coating process, and the perovskite film is prepared by an annealing process (annealing temperature 130°C, annealing time 10 minutes); then, the perovskite film is transferred to a high vacuum evaporation chamber, and TPBi, LiF and Al of the required thickness are prepared in turn by thermal evaporation, and the effective area of ​​the light-emitting device is determined by the area of ​​the Al electrode and the intersection area of ​​the ITO. Finally, the light-emitting device is placed on the top of the integrating sphere, and a source meter is used to apply voltage to both ends of the device and inject current. A spectrometer is used to collect the number of photons after diffuse reflection by the integrating sphere, and the changes in current and photon number with voltage are recorded. Based on the assumption that the light-emitting device is a Lambertian body, parameters such as external quantum efficiency, brightness, luminescence peak, CIE and current efficiency that characterize the performance of the device are obtained.

[0062] The preparation process of perovskite thin film is as follows Figure 1 As shown; the device structure of the light emitting diode is as follows Figure 5 As shown; the corresponding energy level structure except the light-emitting layer is as follows Figure 6 As shown; the performance of the light-emitting diode device based on the grown thin film is shown Fig. 9 shown.

[0063] Example 4

[0064] A light-emitting diode device with a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite as an active layer, specifically, a zero-dimensional-three-dimensional dual-phase all-inorganic perovskite film with a feed chlorine content of 80%. In this embodiment, the feed chlorine content of CsX is 80%. The complete device preparation process is as follows: first, on the ITO surface that has been ultrasonically cleaned with deionized water, acetone, and anhydrous ethanol and plasma-treated, a PEDOT:PSS film is prepared in an open air environment by a spin coating process, and the film preparation is completed by an annealing process (annealing temperature 150°C, annealing time 10 minutes); secondly, on its surface, a PbBr2 film is prepared in an open air environment by a spin coating process, and the film preparation is completed by an annealing process (annealing temperature 70°C, annealing time 10 minutes); then, on the surface of the PbBr2 film, a 20% CsBr+80% CsCl film is prepared in an open air environment by a spin coating process, and the perovskite film is prepared by an annealing process (annealing temperature 130°C, annealing time 10 minutes); then, the perovskite film is transferred to a high vacuum evaporation chamber, and TPBi, LiF and Al of the required thickness are prepared in turn by thermal evaporation, and the effective area of ​​the light-emitting device is determined by the area of ​​the Al electrode and the intersection area of ​​the ITO. Finally, the light-emitting device is placed on the top of the integrating sphere, and a source meter is used to apply voltage to both ends of the device and inject current. A spectrometer is used to collect the number of photons after diffuse reflection by the integrating sphere, and the changes in current and photon number with voltage are recorded. Based on the assumption that the light-emitting device is a Lambertian body, parameters such as external quantum efficiency, brightness, luminescence peak, CIE and current efficiency that characterize the performance of the device are obtained.

[0065] The preparation process of perovskite thin film is as follows Figure 1 As shown; the device structure of the light emitting diode is as follows Figure 5 As shown; the corresponding energy level structure except the light-emitting layer is as follows Figure 6 As shown; the performance of the light-emitting diode device based on the grown thin film is shown Fig.10 shown.

[0066] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a mixed bromine-chlorine all-inorganic perovskite film in a high humidity air environment, characterized in that: The perovskite film prepared by a two-step spin coating process in a high humidity air environment has a zero-dimensional-three-dimensional dual-phase structure and a chemical formula of Cs4Pb(Br 1-x Cl x )6-CsPb(Br 1-x Cl x )3, where 0 <x<1。 2. The preparation method according to claim 1, characterized in that: Tetraphenylphosphonium halide and Tween 20 were added to the spin coating solutions in the first and second steps to restrict the phase growth in the film.

3. The preparation method according to claim 1, characterized in that: The spin-coated film is subjected to thermal annealing in an air environment to assist ion diffusion, and a dual-phase perovskite component is generated under the synergistic effect of tetraphenylphosphine halide and Tween 20.

4. The preparation method according to claim 1, characterized in that: The bandgap of the film can be controlled by adjusting the chloride ion content in the two-step spin coating solution to adjust the emission wavelength from green (x=0) to deep blue (x>0.5).

5. The preparation method according to claim 1, characterized in that: The method specifically comprises the following steps: 1) PbX2, tetraphenylphosphorus halide and Tween 20 are dissolved in DMF in a certain ratio, and heated and stirred in an air environment until all dissolved to obtain a solution A; in an air environment, the solution A is distributed on the surface of the substrate A by a spin coating method to obtain a substrate B; 2) dissolving CsX, tetraphenylphosphorus halide and Tween 20 in a mixed solvent of water and isopropanol in a certain proportion to obtain a solution B, wherein X in CsX is bromine, chlorine or a mixture thereof, and the halogen in tetraphenylphosphorus halide is bromine, chlorine or a combination thereof; distributing the solution B on the surface of the substrate B by spin coating in a high humidity air environment; 3) The obtained PbX2 / CsX double-layer film is subjected to thermal annealing in an air environment to assist ion diffusion across the PbX2 / CsX interface and react to form a dual-phase perovskite.

6. The preparation method according to claim 5, characterized in that: In step 1), the PbX2, tetraphenylphosphorus halide and Tween 20 are dissolved in DMF in a mass ratio of 25:0.1-25:0.1-25.

7. The preparation method according to claim 5, characterized in that: In step 1), the substrate A is any one of a plastic film, a metal sheet, and a glass sheet.

8. The preparation method according to claim 5, characterized in that: In step 2), the CsX, tetraphenylphosphonium halide and Tween 20 are dissolved in a mixed solvent of water and isopropanol in a mass ratio of 8:0.1 to 8:0.1 to 8; the volume ratio of water to isopropanol is less than 1, and the volumes of isopropanol and water are adjusted according to the mass of CsX and the chloride ion content until CsX can just be dissolved.

9. The preparation method according to claim 5, characterized in that: In step 2), the high humidity air environment refers to an air environment with a relative humidity of 40 to 70% rh.

10. Use of the mixed bromine-chlorine all-inorganic perovskite film prepared by the preparation method according to any one of claims 1 to 9 in the preparation of light-emitting diodes, characterized in that: Cs4Pb(Br 1-x Cl x )6-CsPb(Br 1-x Cl x )3 is used as the light-emitting medium of the light-emitting diode, and a transparent bottom electrode / hole or electron transport layer / perovskite light-emitting layer / electron or transport layer / interface modification layer / counter electrode structure is adopted.