Preparation method of full-color OLED

By using peelable photoresist on the substrate of the OLED display to form the shadow mask structure, the problems of edge afterimage and alignment abnormalities caused by metal shadow mask accuracy and gravity sagging are solved, and a more efficient preparation process and a more uniform pixel brightness.

CN118984635APending Publication Date: 2024-11-19广西自贸区睿显科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062083.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the preparation of OLED displays, the accuracy requirements of the metal shadow mask are high and easy to sag due to gravity, resulting in the problems of edge afterimage and alignment abnormalities during the evaporation process.

Method used

A shadow mask structure is formed on the substrate using peelable photoresist, and an evaporation cavity is created through the photolithography process, which solves the accuracy and gravity sagging problems of traditional metal shadow masks, improves processing accuracy and avoids alignment abnormalities.

Benefits of technology

It improves the preparation efficiency and accuracy of OLED displays, reduces edge afterimage, and ensures the uniformity of pixel brightness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984635A_ABST
    Figure CN118984635A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a full-color OLED (Organic Light Emitting Diode), which comprises independent preparation of an RGB (Red, Green, Blue) organic light-emitting multilayer structure on a substrate by adopting an evaporation method, and the preparation method of the full-color OLED comprises the following steps: before the RGB organic light-emitting multilayer structure is prepared by adopting the evaporation method, attaching a peelable photoresist on the substrate, and enabling the RGB light-emitting pixel region corresponding to the photoresist to form a shadow mask structure through a photoetching process, wherein the shadow mask structure is used for evaporating the RGB organic light-emitting multi-layer structure. The shadow mask structure is prepared on the substrate by adopting the peelable photoresist, and compared with a traditional metal shadow mask, the shadow mask structure is higher in machining precision; and the photoresist is directly attached to the substrate, and through the supporting effect of the substrate, the problem that alignment is abnormal due to the fact that a traditional metal shadow mask droops under the action of gravity is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of OLED display manufacturing technology, and in particular to a method for manufacturing a full-color OLED. Background Art

[0002] Among the OLED full-color methods, there are mainly evaporation of RGB independent organic light-emitting materials, inkjet printing of RGB independent organic light-emitting materials, template transfer of RGB independent organic light-emitting materials, OLED white light plus color filter layer, and OLED blue light plus color conversion layer. Among them, the evaporation of RGB independent organic light-emitting materials has become the most mainstream process due to its mature process, extremely high luminous efficiency, and high color purity, but it also has problems such as limited production display size and large pixel size.

[0003] The main reason for the problem is the need to use a high-precision metal shadow mask. The metal shadow mask needs to use a special low-expansion coefficient metal material, which is generally lower than 5ppm / ℃. At the same time, the metal shadow mask has corner problems, which can easily cause edge afterimage problems and uneven pixel brightness. At the same time, in the large-area metal shadow mask evaporation, the metal shadow mask will sag due to gravity when the net is stretched, which in turn causes abnormal alignment. Summary of the invention

[0004] The invention discloses a method for preparing a full-color OLED, which solves the problems in the existing OLED light-emitting element preparation process that the metal shadow mask has high precision requirements and sags due to gravity, resulting in edge afterimages and abnormal alignment during the evaporation process.

[0005] A method for preparing a full-color OLED includes independently preparing an RGB organic light-emitting multilayer structure on a substrate by using a vapor deposition method. Before the RGB organic light-emitting multilayer structure is prepared by using the vapor deposition method, a strippable photoresist is attached to the substrate, and a shadow mask structure is formed in the RGB light-emitting pixel area corresponding to the photoresist through a photolithography process, so as to evaporate the RGB organic light-emitting multilayer structure.

[0006] The present application uses a strippable photoresist to manufacture a shadow mask structure on a substrate, which has higher processing accuracy than a traditional metal shadow mask. The photoresist is directly attached to the substrate, and through the support of the substrate, the problem of the traditional metal shadow mask sagging due to gravity, resulting in abnormal alignment, is solved.

[0007] Several optional methods are also provided below, but they are not intended to be additional limitations on the above-mentioned overall solution, but are merely further supplements or preferences. Under the premise that there are no technical or logical contradictions, each optional method can be combined with the above-mentioned overall solution separately, and multiple optional methods can also be combined.

[0008] Optionally, the strippable photoresist comprises at least a first photoresist layer connected to the substrate and a second photoresist layer located above the first photoresist layer;

[0009] In the photolithography process, a plurality of evaporation cavities corresponding to the RGB light-emitting pixel areas are formed by the difference in reaction rates between the first photoresist layer, the second photoresist layer and the positive developer.

[0010] Optionally, the evaporation chamber includes an evaporation chamber opening located at the second photoresist layer and an evaporation chamber chamber located at the first photoresist layer, the size of the evaporation chamber opening corresponds to the size of a single RGB luminous pixel, and the evaporation chamber chamber is larger than the size of the RGB luminous pixel.

[0011] Optionally, the first photoresist layer is made of non-photosensitive photoresist, and the second photoresist layer is made of positive photoresist.

[0012] Optionally, the above preparation method specifically comprises the following steps:

[0013] S1, taking a substrate, and etching the substrate to form a plurality of anode structures;

[0014] S2, sequentially coating a first photoresist layer and a second photoresist layer on the anode structure, and forming a vapor deposition cavity on the first photoresist layer and the second photoresist layer at corresponding locations of each anode structure through exposure and development operations;

[0015] S3, using an evaporation process to perform evaporation deposition on the substrate with the evaporation cavity in step S2, to obtain an organic light-emitting multilayer structure of a single color on the anode structure;

[0016] S4, using a coating process to deposit a protective layer having a sealing and insulating function on the organic light-emitting multilayer structure;

[0017] S5, immersing the substrate with the protective layer in a post-treatment solution to remove the first photoresist layer and the second photoresist layer on the substrate;

[0018] S6, repeating steps S2 to S5 to complete the preparation of the RGB organic light-emitting multilayer structure;

[0019] S7, etching the substrate after step S6 to remove the protective layer above the RGB organic light-emitting multilayer structure, and forming a cathode layer at one end of the organic light-emitting multilayer structure away from the anode structure by evaporation;

[0020] S8. Using an atomic layer deposition process, the substrate after completing step S6 is packaged to obtain a finished product.

[0021] Optionally, the maximum thickness of the anode structure is 150 nm.

[0022] Optionally, the minimum thickness of the first photoresist layer is 800 nm.

[0023] Optionally, the organic light-emitting multilayer structure includes a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a transparent conductive layer; and the transparent conductive layer is connected to the protective layer.

[0024] Optionally, the coating process in step S4 is a vacuum magnetron sputtering process or an electron beam vacuum evaporation process.

[0025] Optionally, the post-treatment solution is a mixture of one or more of N-methylpyrrolidone, propylene glycol monomethyl ether acetate, methyl ethyl ketone, cyclohexanone, and isopropanol.

[0026] The beneficial effects of this application are as follows:

[0027] 1. The present application manufactures an evaporation cavity on the first photoresist layer and the second photoresist layer by stacking the first photoresist layer and the second photoresist layer. The evaporation cavity has a small mouth and a large chamber, which can be suitable for the evaporation of an organic light-emitting multilayer structure. At the same time, the first photoresist layer provides support for the second photoresist layer to prevent the second photoresist layer from sagging due to gravity, thereby solving the problem of abnormal alignment caused by sagging of a traditional metal shadow mask due to gravity.

[0028] 2. The present application utilizes the difference in reaction rates between the first photoresist layer and the second photoresist layer and the positive developer to make the reaction rate of the first photoresist layer higher than that of the second photoresist layer, thereby quickly obtaining a structure with a small evaporation cavity mouth and a large chamber, thereby improving preparation efficiency.

[0029] 3. The present application achieves the effect of rapidly stripping the photoresist layer by reacting the first photoresist layer, the second photoresist layer and the post-treatment solution.

[0030] 4. The present application sets a transparent conductive layer on the top layer of the organic light-emitting multilayer structure. After the protective layer is removed by dry etching, the transparent conductive layer can protect the electron injection layer located below the transparent conductive layer. Improve the problem of excessive etching causing abnormal electron injection layer due to poor uniformity of the entire etching surface caused by dry etching. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of the structure after the anode structure is prepared in this application;

[0032] Figure 2 It is a schematic diagram of the structure after the shadow mask structure is prepared in this application;

[0033] Figure 3 This is a schematic diagram of the structure after the organic light-emitting multilayer structure is prepared in this application;

[0034] Figure 4 This is a schematic diagram of the structure after the protective layer is prepared in this application;

[0035] Figure 5 This is a schematic diagram of the structure after removing the shadow mask structure in this application;

[0036] Figure 6 This is a schematic diagram of the structure after the organic light-emitting multilayer structure is prepared in this application;

[0037] Figure 7 A schematic diagram of an organic light-emitting multilayer structure after removing the protective layer in this application;

[0038] Figure 8 This is a schematic diagram of the structure after the cathode layer is prepared in this application;

[0039] Fig. 9 This is a schematic structural diagram of the finished OLED light-emitting element of this application.

[0040] The reference numerals in the figures are described as follows:

[0041] 1. Substrate; 2. Anode structure; 3. Shadow mask structure; 31. First photoresist layer; 32. Second photoresist layer; 4. Evaporation chamber; 5. Organic light-emitting multilayer structure; 6. Protective layer; 7. Cathode layer; 8. Atomic layer. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0043] It should be noted that when a component is referred to as being "connected" to another component, it may be directly connected to the other component or there may be a central component. When a component is referred to as being "disposed on" another component, it may be directly disposed on the other component or there may be a central component at the same time.

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0045] refer to Figures 1 to 9In one embodiment of the present application, a method for preparing a full-color OLED is disclosed, including: a first step: etching to form a plurality of anode structures 2 on a substrate 1; a second step: coating a photoresist on the substrate 1 and performing a photolithography process according to the position of the anode structure 2 to obtain a shadow mask structure 3; a third step: using an evaporation process to evaporate an organic light-emitting multilayer structure 5 on the anode structure 2, and removing the photoresist after the organic light-emitting multilayer structure 5 is obtained; a fourth step: using an evaporation process to form a common cathode on the organic light-emitting multilayer structure 5; and a fifth step: using an atomic layer 8 deposition process to encapsulate to obtain a finished product.

[0046] refer to Figure 1 In one embodiment, the anode structure 2 is formed by etching a conductive metal on the substrate 1 by an etching process. The number of anode structures 2 is several and they are distributed in an array on the substrate 1, serving as the positive electrode of the light-emitting element and used to carry RGB organic light-emitting materials. It can be understood that a single anode structure 2 corresponds to a light-emitting pixel on the OLED light-emitting element.

[0047] In order to make the anode structure 2 have high conductivity and high work function, the material of the anode structure 2 can be a mixture of one or more of aluminum (Al), molybdenum (Mo), gold (Au), silver (Ag), platinum (Pt), zinc oxide (ZnO), titanium oxide (TiO2), and ITO (indium tin oxide).

[0048] Furthermore, when the anode structure 2 is stacked with multiple conductive metals, one of gold (Au), silver (Ag), zinc oxide (ZnO), and titanium oxide (TiO2) can be selected as the topmost or outermost material to ensure that the anode structure 2 remains stable during the subsequent preparation process and has relative chemical stability.

[0049] In some embodiments, the anode structure 2 is made by a wet etching process.

[0050] In another embodiment, the anode structure 2 is made by a dry etching process.

[0051] refer to Figure 2 In order to solve the expansion coefficient problem and the corner problem of the existing metal shadow mask, in one embodiment, a shadow mask structure 3 made of photoresist is adopted. The photoresist is coated on the substrate 1 and processed by a photolithography process to obtain a shadow mask structure 3 composed of photoresist and attached to the substrate 1, which is used to replace the metal shadow mask.

[0052] The shadow mask structure 3 made of photoresist has higher precision than the traditional metal shadow mask, and can effectively solve the edge afterimage problem of the organic light-emitting multilayer structure 5 formed in the subsequent evaporation process due to insufficient corner precision.

[0053] The shadow mask structure 3 made of photoresist has a plurality of evaporation cavities 4 corresponding to the anode structure 2, such as Figure 2 As shown, the evaporation chamber 4 has an opening and a chamber, and the anode structure 2 is located in the evaporation chamber 4. The opening of the evaporation chamber 4 is the same size as the single anode structure 2 and is located above the anode structure 2. It can be understood that the projection of the opening of the evaporation chamber 4 along the height direction coincides with the anode structure 2 located in the evaporation chamber 4.

[0054] Furthermore, the evaporation chamber 4 is obtained by drying after exposure and development steps.

[0055] Furthermore, since the organic light-emitting multilayer structures 5 corresponding to the distribution of the three colors RGB need to be evaporated separately, the photoresist is connected to the substrate 1 in a peelable manner.

[0056] In order to correspond to the separate evaporation steps of RGB colors, several anode structures 2 are artificially divided into red pixel area, green pixel area, and blue pixel area, and the first shadow mask structure 3 preparation, the first evaporation, the stripping of the shadow mask structure 3, the second shadow mask structure 3 preparation, the second evaporation, the stripping of the shadow mask structure 3, the third shadow mask structure 3 preparation, the third evaporation, and the stripping of the shadow mask structure 3 are performed to complete the evaporation of the organic light-emitting multilayer structure 5 corresponding to the red, green and blue colors.

[0057] Among them, in the first preparation of the shadow mask structure 3, the second preparation of the shadow mask structure 3, and the third preparation of the shadow mask structure 3, on the shadow mask structures 3 prepared for the three times, the position of the evaporation chamber 4 needs to be adjusted in turn to correspond to the red pixel area, the green pixel area, and the blue pixel area, respectively, so as to realize the evaporation of the organic light-emitting multilayer structure 5 corresponding to the distribution of the RGB three colors.

[0058] refer to Figure 3 In some embodiments, the organic light-emitting multilayer structure 5 is prepared by using an evaporation process, by performing full-surface evaporation on one side of the substrate 1 where the anode structure 2 is located, and shielding it with a shadow mask structure 3 composed of a photoresist, so as to form an organic light-emitting multilayer structure 5 on the anode structure 2.

[0059] Furthermore, the organic light-emitting multilayer structure 5 includes, which are sequentially evaporated: a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a transparent conductive layer.

[0060] The light-emitting layer can be evaporated according to the color currently required, and can be one of a red light-emitting layer, a green light-emitting layer, and a blue light-emitting layer.

[0061] like Figure 6 As shown, Figure 6The reference symbol R represents a red organic light-emitting multilayer structure, the reference symbol G represents a green organic light-emitting multilayer structure, and the reference symbol B represents a blue organic light-emitting multilayer structure.

[0062] It should be noted that, in some embodiments, the above-mentioned strippable photoresist can be understood as: separating the photoresist from the substrate 1 by external force;

[0063] In other embodiments, the above-mentioned strippable photoresist can also be understood as: the photoresist is separated from the substrate 1 through a chemical reaction by immersing in a post-treatment solution.

[0064] The post-treatment solution may be one of N-methylpyrrolidone (NMP), propylene glycol monomethyl ether acetate (PGMEA), methyl ethyl ketone (MEK), cyclohexanone, isopropyl alcohol (IPA) or a mixture thereof.

[0065] Furthermore, when the photoresist is stripped by immersion in a post-treatment solution, in order to protect the organic light-emitting multilayer structure 5 that has been prepared on the substrate 1, a protective layer 6 is provided on the outer layer of the organic light-emitting multilayer structure 5 to isolate the post-treatment solution from contact with the organic light-emitting multilayer structure 5 and avoid reaction between the two.

[0066] refer to Figure 4 In some embodiments, the protective layer 6 can be prepared by using a vacuum magnetron sputtering process or an electron beam vacuum evaporation process, so as to be deposited on the outer surface of the organic light-emitting multilayer structure 5 to form a thin film.

[0067] Furthermore, the protective layer 6 has the function of isolating water and oxygen and has insulating ability, and its material can be one of aluminum oxide (Al2O3), silicon nitride (Si3N4), silicon oxide (SiO2), zirconium oxide (ZrO2), titanium oxide (TiO2), hafnium oxide (HfO2), copper oxide (CuO), tantalum oxide (Ta2O5), and cerium oxide (CeO2).

[0068] To ensure that the protective layer 6 can completely isolate the post-treatment solution, the protective layer 6 needs to fully cover the upper end and side walls of the organic light-emitting multilayer structure 5. Therefore, the chamber of the evaporation chamber 4 in the above embodiment is larger than the size of its opening (such as Figure 2 As shown), a certain distance is provided between the inner wall of the chamber and the anode structure 2 and the organic light-emitting multilayer structure 5, so as to form a protective layer 6 on the side wall of the organic light-emitting multilayer structure 5.

[0069] In some embodiments, the photoresist used to make the shadow mask structure 3 includes at least a first photoresist layer 31 connected to the substrate 1 and a second photoresist layer 32 located above the first photoresist layer 31. The first photoresist layer 31 is made of non-photosensitive photoresist and the second photoresist layer 32 is made of positive photoresist.

[0070] Furthermore, the mouth of the evaporation chamber 4 is located at the second photoresist layer 32, and the chamber of the evaporation chamber 4 is located at the first photoresist layer 31. There is a difference in the reaction rate between the first photoresist layer 31 and the second photoresist layer 32 and the positive developer, and the reaction rate of the first photoresist layer 31 is higher than the reaction rate of the second photoresist layer 32, thereby forming the evaporation chamber 4 with the same size as the anode structure 2 and a certain distance between the inner wall of the chamber and the anode structure 2.

[0071] Meanwhile, the above-mentioned evaporation chamber 4 is made of the first photoresist layer 31 and the second photoresist layer 32. The first photoresist layer 31 can support the second photoresist layer 32, thereby solving the problem that the traditional direct metal shadow mask sags due to gravity when the net is stretched, thereby causing abnormal alignment.

[0072] refer to Figure 7 and Figure 8 In some embodiments, the preparation of the common cathode includes forming a common cathode layer 7 on top of the plurality of organic light-emitting multilayer structures 5 by a full-surface evaporation process.

[0073] Furthermore, if there is a protective layer 6 on the organic light-emitting multilayer structure 5, it is necessary to first remove the protective layer 6 between the organic light-emitting multilayer structure 5 and the cathode layer 7 by dry etching, and then evaporate the organic light-emitting multilayer structure 5 to connect the cathode layer 7 to the transparent conductive layer of the organic light-emitting multilayer structure 5.

[0074] As described above, after the transparent conductive layer is dry-etched to remove the protective layer 6, the electron injection layer below the transparent conductive layer can be protected to ensure the uniformity of the electron injection layer, thereby improving the problem of excessive etching resulting from poor uniformity of the entire surface caused by dry etching, which causes the electron injection layer to become abnormal.

[0075] Furthermore, the transparent conductive layer can be tin oxide, indium oxide, cadmium oxide, cadmium stannate, etc., and a small amount of fluorine and antimony can be added to the above compounds to prepare a transparent conductive film.

[0076] refer to Fig. 9 , using the atomic layer 8 deposition process for encapsulation, forming an atomic layer 8 on the negative electrode layer to complete the preparation of the full-color OLED light-emitting element.

[0077] In some embodiments of the present application, a specific method for preparing a full-color OLED is also disclosed, and the steps are as follows:

[0078] S1. References Figure 1 , taking a substrate 1, and forming a plurality of array-distributed anode structures 2 on a surface of one side of the substrate 1 through a wet etching process;

[0079] In some embodiments, the thickness of a single anode structure 2 is a maximum of 150 nm, preferably 130 nm;

[0080] S2, dividing the anode structure 2 in step S1 into light-emitting areas corresponding to red, green and blue to form a red pixel matrix, a green pixel matrix and a blue pixel matrix;

[0081] S3. Reference Figure 2 , on the side of the substrate 1 where the anode structure 2 is located, non-photosensitive photoresist is sequentially coated to form a first photoresist layer 31, and positive photoresist is coated to form a second photoresist layer 32;

[0082] In some embodiments, the thickness of the first photoresist layer 31 formed by the non-photosensitive photoresist is greater than that of the anode structure 2;

[0083] Furthermore, the thickness of the first photoresist layer 31 is greater than 800 nm, preferably 800 nm, so that the evaporation chamber 4 located on the first photoresist layer 31 has enough space to accommodate the anode structure 2 and other structures subsequently stacked on the anode structure 2;

[0084] S4. References Figure 2 , exposure and development operations are performed in sequence according to the pixel dot matrix corresponding to the color (red, green, blue) currently required to be prepared, and an evaporation cavity 4 corresponding to the pixel dot matrix corresponding to the color currently required to be prepared is prepared on the first photoresist layer 31 and the second photoresist layer 32 to form a shadow mask structure 3;

[0085] S5. Reference Figure 3 , using an evaporation process, evaporating the entire surface of one side of the shadow mask structure 3 on the substrate 1, and evaporating in sequence: a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a transparent conductive layer to obtain an organic light-emitting multilayer structure 5;

[0086] S6. Reference Figure 4 , using a vacuum magnetron sputtering process, coating one side of the shadow mask structure 3 on the substrate 1, and forming a protective layer 6 on the outer side of the organic light-emitting multilayer structure 5;

[0087] S7, Reference Figure 5 , fully immerse the organic light-emitting multilayer structure 5 with the protective layer 6 and the substrate 1 in a post-treatment solution to remove the shadow mask structure 3;

[0088] In some embodiments, the post-treatment solution can react with the first photoresist layer 31 and the second photoresist layer 32 to remove the first photoresist layer 31 and the second photoresist layer 32 at the same time;

[0089] In other embodiments, the post-treatment solution reacts only with the first photoresist layer 31, or reacts with the first photoresist layer 31 at a faster rate, so that the connection between the second photoresist layer 32 and the substrate 1 by the first photoresist layer 31 is lost, and the second photoresist layer 32 and the protective layer 6 on the second photoresist layer 32 fall off;

[0090] S8, forming red, green and blue light-emitting regions as required, repeating steps S4 to S7 until the preparation of the organic light-emitting multilayer structure 5 on the red pixel matrix, the green pixel matrix and the blue pixel matrix is ​​completed (eg Figure 6 shown);

[0091] S9, using dry etching to remove the protective layer 6 (such as Figure 7 shown);

[0092] S10, Reference Figure 8 , using an evaporation process, performing evaporation deposition on the entire side of the substrate 1 where the organic light-emitting multilayer structure 5 is located, to form a common cathode layer 7 on all the organic light-emitting multilayer structures 5;

[0093] S11. Reference Fig. 9 , the atomic layer 8 deposition process is used for packaging, and the atomic layer 8 is formed on the negative electrode layer to complete the preparation of the full-color OLED light-emitting element.

[0094] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. When the technical features in different embodiments are embodied in the same figure, it can be regarded that the figure also discloses the combination examples of the various embodiments involved.

[0095] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A method for preparing a full-color OLED, comprising independently preparing a RGB organic light-emitting multilayer structure on a substrate by an evaporation method, wherein the method for preparing the full-color OLED is characterized in that: Before the evaporation method is used to prepare the RGB organic light-emitting multilayer structure, a strippable photoresist is attached to the substrate, and a shadow mask structure is formed in the RGB light-emitting pixel area corresponding to the photoresist through a photolithography process for evaporating the RGB organic light-emitting multilayer structure.

2. The method for preparing a full-color OLED according to claim 1, characterized in that: The strippable photoresist comprises at least a first photoresist layer connected to the substrate and a second photoresist layer located above the first photoresist layer; In the photolithography process, a plurality of evaporation cavities corresponding to the RGB light-emitting pixel areas are formed by the difference in reaction rates between the first photoresist layer, the second photoresist layer and the positive developer.

3. The method for preparing a full-color OLED according to claim 2, characterized in that: The evaporation chamber includes an evaporation chamber opening located at the second photoresist layer and an evaporation chamber chamber located at the first photoresist layer. The size of the evaporation chamber opening corresponds to the size of a single RGB luminous pixel, and the evaporation chamber chamber is larger than the size of the RGB luminous pixel.

4. The method for preparing a full-color OLED according to claim 3, characterized in that: The first photoresist layer is made of non-photosensitive photoresist, and the second photoresist layer is made of positive photoresist.

5. The method for preparing a full-color OLED according to claim 4, characterized in that: The specific steps include: S1, taking a substrate, and etching the substrate to form a plurality of anode structures; S2, sequentially coating a first photoresist layer and a second photoresist layer on the anode structure, and forming a vapor deposition cavity on the first photoresist layer and the second photoresist layer at corresponding locations of each anode structure through exposure and development operations; S3, using an evaporation process to perform evaporation deposition on the substrate with the evaporation cavity in step S2, to obtain an organic light-emitting multilayer structure of a single color on the anode structure; S4, using a coating process to deposit a protective layer having a sealing and insulating function on the organic light-emitting multilayer structure; S5, immersing the substrate with the protective layer in a post-treatment solution to remove the first photoresist layer and the second photoresist layer on the substrate; S6, repeating steps S2 to S5 to complete the preparation of the RGB organic light-emitting multilayer structure; S7, etching the substrate after step S6 to remove the protective layer above the RGB organic light-emitting multilayer structure, and forming a cathode layer at one end of the organic light-emitting multilayer structure away from the anode structure by evaporation; S8. Using an atomic layer deposition process, the substrate after completing step S6 is packaged to obtain a finished product.

6. The method for preparing a full-color OLED according to claim 5, characterized in that: The maximum thickness of the anode structure is 150 nm.

7. The method for preparing a full-color OLED according to claim 5, characterized in that: The minimum thickness of the first photoresist layer is 800 nm.

8. The method for preparing a full-color OLED according to claim 5, characterized in that: The organic light-emitting multilayer structure comprises a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a transparent conductive layer; the transparent conductive layer is connected to the protective layer.

9. The method for preparing a full-color OLED according to claim 5, characterized in that: The coating process in step S4 is a vacuum magnetron sputtering process or an electron beam vacuum evaporation process.

10. The method for preparing a full-color OLED according to claim 5, characterized in that: The post-treatment solution is a mixed solution of one or more of N-methylpyrrolidone, propylene glycol monomethyl ether acetate, methyl ethyl ketone, cyclohexanone and isopropanol.