Wet mask patterning method of thin film solar cell electrode and thin film solar cell
Through the wet masking technology, the use of selectively dissolved polymer materials and orthogonal solvents is achieved to achieve high efficiency and low damage patterning of thin-film solar cell electrodes, solve the damage problem in the masking process in the prior art, and improve the Energy conversion efficiency of solar cells.
Patent Information
- Application Number
- CN202411070078.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art has problems such as ablation damage, bottom layer damage, microcracks and dimensional changes in the electrode masking process of thin-film solar cells, making it difficult to realize an efficient and low-damage patterned masking method.
Wet mask patterning is performed using selectively dissolved polymer materials, and non-destructive electrode mask patterning is achieved through the combination of vacuum sputtering and orthogonal solvents, which is suitable for a variety of electrode materials and structures.
The accuracy and uniformity of the electrode mask are improved, damage to the active layer by laser marking is avoided, and the energy conversion efficiency of the solar cell is enhanced.
Smart Images

Figure CN118984636A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to an electrode masking method of a thin-film solar cell and an application thereof. Background Art
[0002] Thin-film photovoltaic technology is a hot topic of academic and industrial attention and research. Its solar cell structure usually consists of transparent electrodes, metal electrodes, photoactive layers, hole transport layers and electron transport layers. Sunlight enters the photoactive layer through the transparent electrode, and the active layer material absorbs photons, and photoelectric conversion is achieved through processes such as exciton generation, exciton diffusion, exciton dissociation, charge transfer and charge collection. However, in the process of transitioning from small-area devices in the laboratory to large-size components in practical applications, it is necessary to develop high-quality, low-damage electrode patterning mask methods to reduce efficiency losses. Generally, dry mask processes such as laser scribing methods have high precision, but are also accompanied by various ablation damage challenges, including incomplete ablation, heat-affected zones, bottom layer damage, microcracks, secondary phase formation and residues in the grooves. Similarly, metal mask plates are also widely used in the manufacture of solar cells because this method can ensure simple, stable and low-cost thin-film mask patterns without damaging the underlying materials. However, there are also some defects, such as it is difficult to achieve precise alignment of the mask plate to the pre-mask area, and the mask effect causes displacement and size changes of the electrode. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a wet mask patterning method for thin-film solar cell electrodes and a thin-film solar cell. The present invention uses a polymer that can be selectively dissolved and removed by a solvent as a mask material. First, the electrode pattern of the mask is drawn on the surface of a pre-deposited substrate. After vacuum sputtering the electrode film, an orthogonal solvent is used to selectively remove the polymer and the electrode covering it to obtain the desired electrode pattern. The electrode masking method of the present invention is not only suitable for a variety of electrode materials or structures, but also simple to operate, flexible in changing the mask pattern and line width, and relatively good in accuracy and uniformity of the mask depth. It also avoids damage to the active layer caused by laser scribing, which helps to improve the energy conversion efficiency of solar cells.
[0004] The specific technical solutions adopted by the present invention are as follows:
[0005] In the first aspect, the present invention provides a wet mask patterning method for thin-film solar cell electrodes. In the manufacturing process of thin-film solar cells, after obtaining a surface to be processed on which an electrode needs to be sputtered, firstly, a layer of patterned mask is processed on the surface to be processed using a selectively soluble polymer material, wherein the shape and position of the hollow area in the patterned mask are the same as the shape and position of the electrode to be sputtered; then, the surface to be processed with the patterned mask is vacuum sputtered to form a sputtered material film on the surface of the patterned mask and the surface to be processed in the hollow area; finally, water or alcohol is used as an orthogonal solvent to selectively dissolve the patterned mask without destroying the surface to be processed, thereby removing the patterned mask and the sputtered material film attached to its surface, and retaining the sputtered material film directly sputtered on the surface to be processed as an electrode.
[0006] As a preferred embodiment of the first aspect, the surface to be processed on which the electrode needs to be sputtered is an electron transport layer of a solar cell.
[0007] As a preference of the first aspect above, the selectively soluble polymer material is one or more of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), and polymethyl methacrylate (PMMA).
[0008] As a preferred embodiment of the above-mentioned first aspect, when using the polymer material to process a patterned mask on the surface to be processed, a prefabricated mold is first used to fit the surface to be processed, the area on the mold corresponding to the electrode to be sputtered is not hollowed out while the remaining areas are hollowed out, and then the polymer material is used to coat the surface to be processed after covering the mold. After the polymer material is cured, the mold is removed to obtain a patterned mask.
[0009] As a preferred embodiment of the first aspect, the electrode to be sputtered is a single-layer metal electrode, or a metal electrode with a buffer layer underneath.
[0010] As a preferred embodiment of the above-mentioned first aspect, the sputtering material is at least one of a metal material and a metal oxide material; the metal material includes aluminum, copper, silver or gold; the metal oxide material includes tin oxide, aluminum oxide, nickel oxide, indium tin oxide or tungsten-doped indium tin oxide.
[0011] As a preference of the first aspect above, the orthogonal solvent is water, methanol, ethanol or isopropanol.
[0012] As a preference of the first aspect above, the polymer material is preferably polyvinyl alcohol (PVA), and the orthogonal solvent is preferably isopropanol.
[0013] In a second aspect, the present invention provides a method for manufacturing a thin-film solar cell electrode based on wet mask patterning, which comprises:
[0014] First, laser P1 scribing is performed on the ITO glass surface according to the designed P1 scribing path to cut off the ITO film layer;
[0015] Then, the hole transport layer, active layer and electron transport layer are processed in sequence on the surface of the ITO glass after laser P1 scribing, and then laser P2 scribing is performed according to the designed P2 scribing path to simultaneously scribe the electron transport layer, active layer and hole transport layer;
[0016] Then, the electron transport layer is used as the surface to be processed where the sputtering electrode is required, a patterned mask having the same line pattern as that corresponding to the laser P3 scribing is pre-designed, and an electrode that does not require laser P3 scribing is processed on the surface of the electron transport layer according to the electrode masking method for a thin-film solar cell as described in any one of claims 1 to 6;
[0017] Finally, after the electrodes are processed, laser P4 marking is performed on the device according to the designed P4 marking path to complete the edge cleaning, and the busbars are welded on the electrodes and packaged to form a battery assembly.
[0018] In a third aspect, the present invention provides a thin-film solar cell electrode manufactured by the manufacturing method described in the second aspect above.
[0019] The present invention uses a type of polymer that can be selectively dissolved and removed by solvents as a mask material, and successively implements a non-destructive or low-damage electrode mask patterning preparation method through vacuum sputtering coating and erasing with solvents such as water and ethanol. This masking method is not only applicable to a variety of electrode materials or structures, but also simple to operate, flexible in changing mask patterns and line widths, and relatively good in accuracy and uniformity of mask depth. It can also be applied to the construction of thin-film solar cells, avoiding damage to the active layer caused by laser scribing, etc., and helping to improve the energy conversion efficiency of solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the structure of a thin-film solar cell.
[0021] Figure 2 Schematic diagram of the electrode mask for testing film thickness at 12 points in Example 1.
[0022] Figure 3 Schematic diagram of the mask pattern and line width of the thin-film solar cell electrode in Example 2.
[0023] Figure 4 Schematic diagram of the electrode mask of the thin-film solar cell assembly in Example 3.
[0024] Figure 5 This is the step profiler height curve of the electrode mask thickness in Example 1.
[0025] Figure 6This is the current-voltage curve of the thin-film solar cell in Example 2.
[0026] Figure 7 This is the current-voltage curve of the thin-film solar cell assembly in Example 3. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation mode of the present invention is described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below. The technical features in each embodiment of the present invention can be combined accordingly without conflicting with each other.
[0028] The present invention provides a wet mask patterning method for thin-film solar cell electrodes, and the specific method is as follows: in the manufacturing process of thin-film solar cells, after obtaining a surface to be processed on which an electrode needs to be sputtered, firstly a layer of patterned mask is processed on the surface to be processed using a selectively soluble polymer material, wherein the shape and position of a hollow area in the patterned mask are the same as the shape and position of the electrode to be sputtered; then vacuum sputtering is performed on the surface to be processed with the patterned mask, and a sputtered material film is formed on the surface of the patterned mask and the surface to be processed in the hollow area; finally, water or alcohol is used as an orthogonal solvent to selectively dissolve the patterned mask without destroying the surface to be processed, and the patterned mask and the sputtered material film attached to the surface are removed, and the sputtered material film directly sputtered on the surface to be processed is retained as the electrode.
[0029] It should be noted that the specific shape of the patterned mask corresponds to the shape of the electrode to be sputtered, and needs to be processed according to the actual situation of the electrode to be sputtered. The present invention does not limit a specific pattern.
[0030] The polymer material used to process the patterned mask in the present invention is a polymer that can be selectively dissolved by an orthogonal solvent when necessary, and the orthogonality of the orthogonal solvent is reflected in that it should be able to dissolve the polymer but will not react to generate other additional components, thereby efficiently and completely removing the patterned mask and the sputtered material film attached to its surface. Moreover, since the orthogonal solvent will also contact the surface to be processed during the process of dissolving the patterned mask, the orthogonal solvent should also ensure that it will not corrode the surface to be processed or react with the components in the surface to be processed. Therefore, the polymer material and the orthogonal solvent should be reasonably selected and optimized considering the materials and process links used in the processing of thin-film solar cells.
[0031] In an embodiment of the present invention, the selectively soluble polymer material is preferably one or more of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), and polymethyl methacrylate (PMMA). The orthogonal solvent is preferably water, methanol, ethanol or isopropanol. In subsequent embodiments of the present invention, the polymer material is preferably polyvinyl alcohol (PVA) and the orthogonal solvent is isopropanol. However, it should be noted that these combinations are only some preferred solutions obtained by screening. In theory, other polymer materials and orthogonal solvents that can achieve similar functions are also feasible.
[0032] It should also be noted that when using polymer materials to process patterned masks on the surface to be processed, if the processing accuracy requirements are not high, the machine can be used to apply the coating as accurately as possible. However, in scenarios where the processing accuracy requirements are high, it is best to pre-manufacture the corresponding mold, and the area corresponding to the electrode to be sputtered on the mold is not hollowed out while the rest of the area is hollowed out. Therefore, when actually processing the patterned mask, the prefabricated mold can be first used to fit the surface to be processed. At this time, the area of the electrode to be sputtered is covered by the mold, while the rest of the area is exposed, and then the polymer material is further used to coat the surface to be processed after covering the mold, so that the mold surface and the surface to be processed below the hollowed-out area of the mold are coated with a layer of polymer material. After the polymer material is solidified, the mold is removed to obtain a patterned mask. At this time, only the area of the electrode to be sputtered that was originally covered by the mold on the surface to be processed is not masked, and the rest of the area is covered with a mask. During subsequent vacuum sputtering, the electrode to be sputtered without a mask will directly form a layer of sputtering material on the surface to be processed. Although a layer of sputtered material will also be formed on other masks, when the polymer material corresponding to the mask is dissolved by the orthogonal solvent, the sputtered material above the mask will also be peeled off, but the sputtered material layer directly attached to the surface to be processed will still remain.
[0033] The wet mask patterning method of the present invention has two main application scenarios in thin-film solar cells. One is to make a mask directly on blank glass to measure the film thickness and its uniformity. The other is to replace the back electrode laser scribing operation in the battery module to reduce or avoid damage to the active layer and improve the battery efficiency.
[0034] For the first application scenario, the surface to be processed that requires sputtering electrodes is a blank glass surface; and for the second application scenario, the surface to be processed that requires sputtering electrodes is the electron transport layer of the solar cell.
[0035] Figure 1The conventional structure of thin-film solar cells is shown. From the perspective of the structure of thin-film solar cells, they are mainly composed of the following layers on a glass substrate: bottom electrode (such as indium tin oxide ITO in the figure, or metals such as Ag), hole transport layer (such as PEDOT:PSS, etc.), active layer (such as donor PM6 / acceptor L8), electron transport layer (such as C60), buffer layer (such as SnOx) and metal electrode layer (such as Ag, TCO film, etc., as the upper electrode). As an important step in forming a solar cell module, the scribing operation plays a role in dividing it into small sub-cell modules and connecting them in series. Among them, P1 scribing is to cut off the bottom electrode, P2 is from the active layer to the bottom electrode, P3 is from the upper electrode to the active layer, and P4 is from the upper electrode to the bottom electrode, which has the effect of clearing the edge. At present, the laser scribing method is mostly used, but the active layer can be easily damaged if the P3 scribing is not done carefully. Therefore, the wet mask method in the present invention can be used to replace the P3 scribing to directly process the upper electrode without the need for P3 scribing, which has the advantage of low damage.
[0036] It should be noted that the electrodes to be sputtered in the present invention need to be adjusted according to the structure of the thin-film solar cell actually processed. Figure 1 In the thin-film solar cell structure, there is a buffer layer and a metal electrode layer above the electron transport layer. Therefore, for such a metal electrode with a buffer layer underneath, the method of the present invention can be sequentially sputtered on the basis of a patterned mask. Of course, in other thin-film solar cell structures, there may be only a single layer of metal electrode above the electron transport layer. Therefore, it is only necessary to sputter a single layer of metal electrode layer on the basis of the patterned mask.
[0037] Therefore, based on the above-mentioned thin-film solar cell electrode mask method, another embodiment of the present invention can also provide a thin-film solar cell electrode manufacturing method based on wet mask patterning, and the specific steps are as follows:
[0038] First, laser P1 scribing is performed on the ITO glass surface according to the designed P1 scribing path to cut off the ITO film layer;
[0039] Then, the hole transport layer, active layer and electron transport layer are processed in sequence on the surface of the ITO glass after laser P1 scribing, and then laser P2 scribing is performed according to the designed P2 scribing path to simultaneously scribe the electron transport layer, active layer and hole transport layer;
[0040] Then, the electron transport layer is used as the surface to be processed where the sputtering electrode is required, a patterned mask having the same line pattern as that corresponding to the laser P3 scribing is pre-designed, and an electrode that does not require laser P3 scribing is processed on the surface of the electron transport layer according to the electrode masking method of the thin-film solar cell described above;
[0041] Finally, after the electrodes are processed, laser P4 marking is performed on the device according to the designed P4 marking path to complete the edge cleaning, and the busbars are welded on the electrodes and packaged to form a battery assembly.
[0042] In the above embodiments of the present invention, specific process parameters and materials can be adjusted as needed. For example, the electrode material or electrode structure of the mask can be changed, and can be at least one of a metal material and a metal oxide material, that is, the electrode can be a metal electrode or a metal oxide electrode. Metal materials include aluminum, copper, silver or gold, etc.; metal oxide materials include tin oxide, aluminum oxide, nickel oxide, indium tin oxide or tungsten-doped indium tin oxide, etc. Generally speaking, the line pattern corresponding to the laser P3 scribing is the boundary line separating different sub-battery modules. The line pattern of the laser P3 scribing is pre-set in the traditional processing method. In the present invention, there is no need to perform laser P3 scribing, so the original line pattern of the laser P3 scribing can be converted into a corresponding patterned mask, and the pattern shapes of the two must be consistent. If a mold is used to process a patterned mask, the pattern in the mold can be processed to be consistent with the line pattern of the laser P3 scribing. Similarly, the line width of the electrode mask can also be adjusted, and the mask line width is generally in the range of 10 to 1000 microns.
[0043] The specific implementation and technical effects of the present invention are described below through several embodiments.
[0044] Example 1
[0045] A blank glass of 300mm×400mm size was cleaned with a cleaning agent, deionized water, acetone, isopropanol and ethanol by ultrasonic oscillation for 30 minutes, dried with a nitrogen stream, and then treated with ultraviolet and ozone plasma for 5 minutes. Polyvinyl alcohol (PVA) was used as a polymer mask material that could be selectively dissolved and removed, and a mold was used to draw the electrode pattern that needed to be masked on the glass surface. Then, a 25nm tin oxide film was first plated using a vacuum coating device, and then a 75nm thick copper electrode was plated. Finally, an orthogonal solvent such as ethanol was used to erase the mask area to obtain the required mask pattern, and the accuracy and uniformity of the plated electrode film thickness were tested using a step profiler (such as Figure 2 shown).
[0046] Example 2
[0047] 1) First, a 15mm×15mm transparent conductive glass with strips of indium tin oxide ITO etched on the surface was cleaned with a detergent, deionized water, acetone, isopropanol and ethanol ultrasonically for 30 minutes, dried with a nitrogen stream, and then treated with ultraviolet and ozone plasma for 5 minutes. Then, the donor PM6 and the acceptor L8 were weighed in a weight ratio of 1:1.2, and a certain volume of toluene solvent was added to prepare an active layer solution with a concentration of 18-22 mg / ml. Then, an equal volume of pure water was added to the PEDOT:PSS solution and stirred at room temperature for one to two hours to prepare a hole transport layer solution.
[0048] 2) Then, a certain amount of PEDOT:PSS solution was transferred to the ITO glass surface by a pipette gun, and annealed at 150°C for 20 minutes after spin coating. Then, the active layer solution was spin-coated on the hole transport layer surface by a pipette gun and heated at 80°C for 5 minutes to form an active layer. Then, an electron transport layer was formed by evaporating C60 on the basis of the active layer.
[0049] 3) Finally, polyvinyl alcohol (PVA) is used as a polymer mask material that can be selectively dissolved and removed, and a patterned mask (such as Figure 3 As shown, the black area is the hollow area covered by the mask, and the gray area is the hollow area), a 100nm thick silver electrode is evaporated on the patterned mask and the electron transport layer exposed in the hollow area of the mask. After the evaporation, ethanol is used as an orthogonal solvent to erase the patterned mask of PVA material and the silver electrode on the surface of the mask, while the silver electrodes in the remaining areas are retained.
[0050] Example 3
[0051] 1) First, the 60mm×60mm ITO glass was cleaned with a cleaning agent, deionized water, acetone, isopropanol and ethanol in turn by ultrasonic oscillation for 30 minutes, dried with a nitrogen stream, and then treated with ultraviolet and ozone plasma for 5 minutes before use. Then the donor PM6 and the acceptor L8 were weighed according to a weight ratio of 1:1.2, and a certain volume of toluene solvent was added to prepare an active layer solution with a concentration of 7mg / ml. Then, an equal volume of pure water was added to the PEDOT:PSS solution and stirred at room temperature for one to two hours to prepare a hole transport layer solution. A methanol dispersion of tin oxide (SnOx) nanoparticles was prepared as an electron transport layer solution.
[0052] 2) Then, the ITO glass is taken out, and laser P1 scribing is performed according to the designed P1 scribing path. After the ITO film layer is cut, a coating operation is performed using a coating machine. The prepared hole transport layer solution, active layer solution and electron transport layer solution are sequentially scraped on the surface of the ITO glass after P1 scribing and annealed for a period of time to form a hole transport layer, an active layer and an electron transport layer. Then, laser P2 scribing is performed according to the designed P2 scribing path, from the electron transport layer to the bottom electrode ITO film layer, so that the electron transport layer, the active layer and the hole transport layer are cut at the same time.
[0053] 3) Finally, referring to the scribing position of P2, polyvinyl alcohol (PVA) is used as a polymer mask material that can be selectively dissolved and removed, and a patterned mask with a strip-shaped hollow mold with a line width of 50 microns is used to draw a patterned mask with a strip-shaped mask on the surface of the electron transport layer. The pattern of the patterned mask is the same as the line pattern that needs to be formed by laser P3 scribing in the traditional processing method. The original 50-micron line width scribing position corresponds to a 50-micron line width PVA material mask, thereby replacing the laser P3 scribing. Then, a 20nm thick tin oxide buffer layer film and a 100nm thick copper electrode are sequentially plated on the patterned mask and the electron transport layer exposed in the mask hollow area using vacuum coating equipment, and then ethanol is used as an orthogonal solvent to erase the PVA material mask and the tin oxide buffer layer film and copper electrode attached to its surface, while the tin oxide buffer layer film and copper electrode in the remaining area are retained as the final upper electrode. Finally, the device after ethanol erasure is cleaned by laser P4 scribing, bus bars are welded on both sides of the upper electrode and packaged to form a battery assembly for subsequent testing (such as Figure 4 shown).
[0054] The test results of the above embodiments 1 to 3 are analyzed as follows:
[0055] In order to ensure the measurement accuracy and uniformity of the thickness of the mask electrode (25nm tin oxide plus 75nm copper electrode) in Example 1, 12 points were selected for testing. The result of one exemplary point is as follows: Figure 5 The total thickness is 100 nm as shown in the step profiler height curve, and the film thickness uniformity at 12 points is within 3%, which shows that the wet masking method of the present invention can still ensure that the prepared electrode film has good uniformity.
[0056] At a light intensity of 100 mW / cm 2 The current-voltage curves of the solar cells in Example 2 and Example 3 were tested under AM 1.5G simulated sunlight. The open circuit voltage of the 15mm×15mm device obtained in Example 2 was 0.83V, and the short circuit current density was 24.48 / cm 2, the filling factor is 0.72, and the photoelectric energy conversion efficiency is 14.78% (such as Figure 6 As shown); the open circuit voltage of the 60mm×60mm device obtained in Example 3 is 5.77V, the current is 68.71mA, the fill factor is 0.70, and the photoelectric energy conversion efficiency is 14.75% (as shown Figure 7 shown).
[0057] It can be seen that the wet mask method can not only be used for simple electrode masks to obtain more precise mask thickness and ideal film thickness uniformity, but can also replace laser scribing and be used in the preparation of thin-film solar cell devices or components, avoiding damage to the active layer caused by laser scribing, which is beneficial to improving the photoelectric energy conversion efficiency of the device.
[0058] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A wet mask patterning method for thin film solar cell electrodes, characterized in that: In the manufacturing process of thin-film solar cells, after obtaining a surface to be processed that requires sputtering electrodes, first, a layer of patterned mask is processed on the surface to be processed using a selectively soluble polymer material, and the shape and position of the hollow area in the patterned mask are the same as the shape and position of the electrode to be sputtered; then, the surface to be processed with the patterned mask is vacuum sputtered to form a sputtered material film on the surface of the patterned mask and the surface to be processed in the hollow area; finally, water or alcohol is used as an orthogonal solvent to selectively dissolve the patterned mask without destroying the surface to be processed, remove the patterned mask and the sputtered material film attached to its surface, and retain the sputtered material film directly sputtered on the surface to be processed as an electrode.
2. The wet mask patterning method for thin-film solar cell electrodes according to claim 1, characterized in that: The surface to be processed which needs to be sputtered with electrodes is the electron transport layer of the solar cell.
3. The electrode masking method of a thin film solar cell according to claim 1, characterized in that: The selectively soluble polymer material is one or more of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), and polymethyl methacrylate (PMMA).
4. The electrode masking method of a thin film solar cell according to claim 1, characterized in that: When the polymer material is used to process a patterned mask on the surface to be processed, a prefabricated mold is first used to fit the surface to be processed, the area on the mold corresponding to the electrode to be sputtered is not hollowed out while the remaining areas are hollowed out, and then the polymer material is used to coat the surface to be processed after covering the mold. After the polymer material is cured, the mold is removed to obtain a patterned mask.
5. The electrode masking method of a thin film solar cell according to claim 1, characterized in that: The electrode to be sputtered is a single-layer metal electrode, or a metal electrode with a buffer layer underneath.
6. The electrode masking method for thin-film solar cells according to claim 1, characterized in that: The sputtering material is at least one of a metal material and a metal oxide material; the metal material includes aluminum, copper, silver or gold; the metal oxide material includes tin oxide, aluminum oxide, nickel oxide, indium tin oxide or tungsten-doped indium tin oxide.
7. The electrode masking method of a thin film solar cell according to claim 1, characterized in that: The orthogonal solvent is water, methanol, ethanol or isopropanol.
8. The electrode masking method for thin-film solar cells according to claim 1, characterized in that: The polymer material is preferably polyvinyl alcohol (PVA), and the orthogonal solvent is preferably isopropanol.
9. A method for manufacturing thin-film solar cell electrodes based on wet mask patterning, characterized in that: include: First, laser P1 scribing is performed on the ITO glass surface according to the designed P1 scribing path to cut off the ITO film layer; Then, the hole transport layer, active layer and electron transport layer are processed in sequence on the surface of the ITO glass after laser P1 scribing, and then laser P2 scribing is performed according to the designed P2 scribing path to simultaneously scribe the electron transport layer, active layer and hole transport layer; Then, the electron transport layer is used as the surface to be processed where the sputtering electrode is required, a patterned mask having the same line pattern as that corresponding to the laser P3 scribing is pre-designed, and an electrode that does not require laser P3 scribing is processed on the surface of the electron transport layer according to the electrode masking method for a thin-film solar cell as described in any one of claims 1 to 6; Finally, after the electrodes are processed, laser P4 marking is performed on the device according to the designed P4 marking path to complete the edge cleaning, and the busbars are welded on the electrodes and packaged to form a battery assembly.
10. A thin-film solar cell electrode manufactured by the manufacturing method according to claim 9.
Citation Information
Cited By
Organic solar cell module preparation method based on P1 groove filling technology
CN122497260A