Resin composition and hot melt adhesive composition

By adjusting the ratio of polyolefin resin, acid modified polyolefin resin, tackifier and filler in the resin composition, the problem of insufficient resin fluidity and water vapor barrier properties in low-pressure forming is solved, and high efficiency of electrical and electronic components is achieved Sealing and waterproofing.

CN118984855APending Publication Date: 2024-11-19TOYOBO MC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033436.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-08
Filing Date
2023-06-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to maintain the fluidity and water vapor barrier properties of the resin in low pressure forming, especially in sealing applications of electrical and electronic components, where adhesion is insufficient and water vapor penetration cannot be effectively prevented.

Method used

The resin composition consisting of polyolefin resin, acid modified polyolefin resin, tackifier and filler is adopted. The specific content ratio is 49-70% of polyolefin resin, 1-30% of acid modified polyolefin resin, and tackifier 10-50%, filler 1-13% to improve the fluidity, adhesion and water vapor barrier properties of the resin.

Benefits of technology

The excellent fluidity and adhesion of the resin composition are achieved, while significantly improving the water vapor barrier properties, making it suitable for electrical and electronic component sealing materials with high waterproofing requirements, and especially for hot melt adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005077844810000141
    Figure BDA0005077844810000141
  • Figure HDA0005077844820000011
    Figure HDA0005077844820000011
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resin composition having excellent water vapor barrier properties while maintaining the fluidity and adhesiveness of a resin that is excellent in low-pressure molding. A resin composition characterized by containing a polyolefin resin (A), an acid-modified polyolefin resin (B), a tackifier (C), and a filler (D), the tackifier (C) content being 10-50 parts by mass and the filler (D) content being 1-13 parts by mass when the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B), and the tackifier (C) is taken as 100 parts by mass, and the filler (D) being plate-shaped.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, and more particularly to a resin composition and a hot melt adhesive composition having excellent fluidity, adhesion and water vapor barrier properties. Background Art

[0002] As insulating resins used for sealing electrical and electronic components used in automobiles, electrical appliances, etc., two-component curing epoxy resins and silicone resins are generally used. However, since a long process is required and the electrical and electronic components may sometimes be damaged due to shrinkage stress during curing, in recent years, low-pressure molding to seal electrical and electronic components using thermoplastic resins has become known.

[0003] From the viewpoints of electrical insulation, water resistance, durability, and melt viscosity, polyester resin is used as a preferred material as a sealing resin for electrical and electronic components. However, in low-temperature and low-pressure molding to reduce damage to electrical and electronic components, the adhesion between the electrical and electronic components and the sealing resin becomes insufficient, and the electrical insulation and water resistance as the target are often not fully exerted. Therefore, from the viewpoint of improving the level of adhesion, attempts to mix a tackifier having a functional group are being actively studied (e.g., Patent Document 1). [Prior art literature] [Patent Literature]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 2004-210893 Summary of the invention [Problems to be solved by the invention]

[0005] In recent years, in addition to the above-mentioned required physical properties, high water vapor barrier properties are also required for electrical and electronic components. However, when a thermoplastic resin mixed with a tackifier is used as in Patent Document 1, although the adhesiveness is improved, there is a problem that the water vapor barrier properties cannot be ensured. In the prior art, there has not been proposed a sealing resin composition that can achieve both water vapor barrier properties while maintaining the fluidity of the resin that is excellent in low-pressure molding.

[0006] The present invention is based on the problems of the prior art. Specifically, the present invention aims to provide a resin composition having excellent water vapor barrier properties while maintaining the fluidity and adhesiveness of a resin excellent in low-pressure molding.

Methods to solve the problem

[0007] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by the following means, thereby completing the present invention. That is, the present invention is constituted by the following contents.

[0008] [1] A resin composition, characterized in that it contains a polyolefin resin (A), an acid-modified polyolefin resin (B), a tackifier (C) and a filler (D), wherein when the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B) and the tackifier (C) is 100 parts by mass, the content of the tackifier (C) is 10 to 50 parts by mass, the content of the filler (D) is 1 to 13 parts by mass, and the filler (D) is in a plate-like shape. [2] The resin composition according to the above [1], wherein the polyolefin resin (A) comprises a polypropylene resin and further comprises at least one of an ethylene-α-olefin copolymer and a propylene-α-olefin copolymer. [3] The resin composition according to [1] or [2] above, wherein the acid-modified polyolefin resin (B) has a melting point of 100° C. or higher. [4] The resin composition according to any one of [1] to [3] above, wherein the tackifier (C) has a hydroxyl value of 1 to 100 KOHmg / g. [5] A resin composition according to any one of [1] to [4] above, wherein, when the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B) and the tackifier (C) is 100 parts by mass, the content of the polyolefin resin (A) is 49 to 70 parts by mass, and the content of the acid-modified polyolefin resin (B) is 1 to 30 parts by mass. [6] A hot melt adhesive composition comprising the resin composition according to any one of [1] to [5] above. [Effects of the invention]

[0009] The resin composition of the present invention exhibits excellent fluidity and adhesion, and further has excellent water vapor barrier properties. Therefore, by using it as a sealing material for products that require high waterproofness, products that meet water vapor barrier properties can be manufactured. In particular, the resin composition of the present invention can be used as a hot melt adhesive, and is particularly suitable for sealing electrical and electronic components. BRIEF DESCRIPTION OF THE DRAWINGS

[0010]

Figure 1

[0011] The present invention is described in detail below.

[0012] <Polyolefin resin (A)> The resin composition of the present invention contains a polyolefin resin (A). By containing the polyolefin resin (A), the resin composition can be given good water vapor barrier properties. The polyolefin resin (A) used in the present invention is not particularly limited, and from the viewpoint of water vapor barrier properties, polypropylene resin is preferred. In addition, from the viewpoint of adhesion to metals and films, ethylene-α-olefin copolymers and propylene-α-olefin copolymers are preferred. In order to highly take into account both water vapor barrier properties and adhesion, polypropylene resins and ethylene-α-olefin copolymers and propylene-α-olefin copolymers can also be used in combination. Here, the polypropylene resin refers to: a so-called homopolypropylene mainly composed of propylene units, does not contain copolymer components such as α-olefins other than propylene, or even if it contains, it is only a very small amount of up to about 1 mol%. In addition, the polyolefin resin (A) refers to a substance that has not been acid-modified, and the acid-modified polyolefin resin (B) described below does not belong to this.

[0013] When a polypropylene resin and an ethylene-α-olefin copolymer and / or a propylene-α-olefin copolymer (hereinafter collectively referred to as an olefin copolymer) are used in combination, the preferred mixing ratio of the polypropylene resin / olefin copolymer is 20 / 80 to 80 / 20, more preferably 30 / 70 to 70 / 30, and further preferably 40 / 60 to 60 / 40 in terms of mass ratio.

[0014] When the total amount of polyolefin resin (A), acid-modified polyolefin resin (B) and tackifier (C) is set to 100 parts by mass, the content of polyolefin resin (A) in the resin composition of the present invention is preferably 49 parts by mass or more, more preferably 50 parts by mass or more, and further preferably 55 parts by mass or more. In addition, it is preferably 70 parts by mass or less, more preferably 65 parts by mass or less, and further preferably 60 parts by mass or less. When the content ratio of polyolefin resin (A) is above the above lower limit, it becomes easy to give the resin composition good water vapor barrier properties. In addition, by making the content ratio of polyolefin resin (A) below the above upper limit, the heat shock resistance of the resin composition becomes good.

[0015] The polyolefin resin (A) used in the present invention preferably has a melt flow rate (hereinafter sometimes referred to as MFR) measured according to JIS K7210-1: 2014 (test temperature 190°C, nominal load 2.16 kg) of 10 to 70 g / 10 minutes. When the MFR is less than 10 g / 10 minutes, the melt viscosity is too high, so the fluidity of the resin is reduced and the moldability may be impaired. When the MFR is more than 70 g / 10 minutes, the viscosity is low, and the resin composition is very easy to soften, and the mechanical properties may be deteriorated. When the polyolefin resin (A) includes a plurality of polyolefin resins, it is preferred that each polyolefin resin is within the above range.

[0016] When the resin composition of the present invention is used as a hot melt adhesive, in order to mold without thermal degradation of the resin as much as possible, it is required to melt rapidly at 210 to 240°C, and it is ideal that the upper limit of the melting point of the polyolefin resin (A) is 210°C. It is preferably below 200°C, and more preferably below 190°C. The lower limit is preferably above 90°C, more preferably above 100°C, further preferably above 110°C, and particularly preferably above 120°C. It is preferably set to be 5 to 10°C higher than the heat-resistant temperature required in the corresponding application. When the polyolefin resin (A) contains a plurality of polyolefin resins, it is preferred that each polyolefin resin is within the above range.

[0017] <Acid-modified polyolefin resin (B)> The resin composition of the present invention contains an acid-modified polyolefin resin (B). By containing the acid-modified polyolefin resin (B), good compatibility can be imparted between the polyolefin resin (A) and the tackifier (C) and the filler (D), and as a result, appropriate fluidity, adhesion, and water vapor barrier properties can be imparted to the resin composition. The acid-modified polyolefin resin (B) is not particularly limited, as long as it is a resin having a polyolefin segment and a carboxylic acid segment, for example, ethylene-unsaturated carboxylic acid copolymers such as ethylene-vinyl acetate-maleic anhydride terpolymer and ethylene-ethyl acrylate-maleic anhydride terpolymer, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified propylene-α-olefin copolymers and other unsaturated carboxylic acid grafted modified polyolefin resins, etc. Among them, maleic anhydride-modified polypropylene can be cited as a preferred acid-modified polyolefin resin.

[0018] The melting point of the acid-modified polyolefin resin (B) used in the present invention is preferably 100° C. or higher, more preferably 110° C. or higher, and further preferably 120° C. or higher. In addition, it is preferably 160° C. or lower, and more preferably 150° C. or lower. If the melting point of the acid-modified polyolefin resin (B) is at least the above lower limit, the heat resistance of the resin composition is good, and if it is at most the above upper limit, the fluidity of the resin composition during molding becomes good.

[0019] When the total amount of polyolefin resin (A), acid-modified polyolefin resin (B) and tackifier (C) is set to 100 parts by mass, the content of the acid-modified polyolefin resin (B) in the resin composition of the present invention is preferably more than 1 part by mass, more preferably more than 3 parts by mass, and further preferably more than 5 parts by mass. In addition, preferably less than 30 parts by mass, more preferably less than 25 parts by mass, and further preferably less than 20 parts by mass. When the content ratio of the acid-modified polyolefin resin (B) is above the above lower limit, the compatibility of the polyolefin resin (A) with the tackifier (C) and the filler (D) becomes good. In addition, when the content ratio of the acid-modified polyolefin resin (B) is below the above upper limit, the formability and mechanical properties become good.

[0020] <Thickener (C)> The resin composition of the present invention contains a tackifier (C). By containing a tackifier (C), when the resin composition is used as a sealant, in addition to being able to impart good adhesion, the fluidity of the resin composition can also be appropriately improved. The tackifier (C) used in the present invention is not particularly limited, and phenol compounds, xylene-modified phenolic resins, terpene-modified phenolic resins, hydrogenated terpene-modified phenolic resins, etc. can be used. In particular, from the viewpoint of compatibility with the polyolefin resin (A), xylene-modified phenolic resins and terpene-modified phenolic resins are preferred.

[0021] The tackifier (C) used in the present invention preferably has a hydroxyl group. By making the tackifier (C) have a hydroxyl group, it is possible to exert an effect of improving the wettability to the substrate, improve the adhesion to the substrate, and improve the insulation. The hydroxyl value of the tackifier (C) is preferably 1KOHmg / g or more, more preferably 30KOHmg / g or more, and further preferably 50KOHmg / g or more. In addition, it is preferably 100KOHmg / g or less, more preferably 90KOHmg / g or less, further preferably 80KOHmg / g or less, and particularly preferably 70KOHmg / g or less. When the hydroxyl value is below the above upper limit, it is possible to maintain appropriate moisture permeability while improving adhesion.

[0022] When the total amount of polyolefin resin (A), acid-modified polyolefin resin (B) and tackifier (C) is set to 100 parts by mass, the content of tackifier (C) in the resin composition of the present invention is preferably more than 10 parts by mass, more preferably more than 20 parts by mass. In addition, preferably less than 50 parts by mass, more preferably less than 40 parts by mass, further preferably less than 30 parts by mass. When the content of tackifier (C) is within the above range, it is possible to show particularly good adhesion. In addition, the flexibility of the resin composition can be suppressed to reduce, the adhesion caused by embrittlement, etc.

[0023] <Filler (D)> The resin composition of the present invention contains a filler (D). By containing a filler (D), it is possible to give the resin composition good water vapor barrier properties. The filler (D) used in the present invention is not particularly limited, and glass beads, calcium carbonate, kaolin, talc, glass fiber, carbon fiber, clay, etc. can be used. In particular, from the viewpoint of improving water vapor barrier properties, the filler (D) used in the present invention is preferably plate-shaped. Here, plate-shaped refers to a plate-like shape with a very small height compared to the width and depth of the filler. The aspect ratio of the filler (D), that is, the ratio of the short diameter to the long diameter of the filler (D) (long diameter / short diameter) is preferably 3 to 500. The aspect ratio of the filler (D) can also be 5 or more, 10 or more, 20 or more, 50 or more, 100 or more, and in addition, it can also be 450 or less, 400 or less, 350 or less, 300 or less, 200 or less. The aspect ratio of the filler (D) can be obtained by methods such as automatic area measurement of an image obtained by observing the filler (D) with an electron microscope. When the aspect ratio of the filler (D) is too low, the water vapor barrier properties may be reduced, and when the aspect ratio is too high, the dispersibility may be deteriorated, and the mechanical properties may be reduced.

[0024] When the total amount of polyolefin resin (A), acid-modified polyolefin resin (B) and tackifier (C) is set to 100 parts by mass, the content of filler (D) in the resin composition of the present invention is preferably more than 1 part by mass, more preferably more than 3 parts by mass, and more preferably more than 5 parts by mass. When the content of filler (D) is above the above lower limit, water vapor barrier becomes good. In addition, sometimes the mechanical properties of the resin composition become good, and the shear bond strength improves. In addition, the content of filler (D) is preferably less than 13 parts by mass, more preferably less than 10 parts by mass, and more preferably less than 8 parts by mass. If the content of filler (D) is below the above upper limit, adhesion becomes good.

[0025] The particle size (D50) of the filler (D) in the resin composition of the present invention is not particularly limited, and may be 1 to 100 μm. The particle size (D50) can generally be measured by a laser diffraction method or a dynamic light scattering method.

[0026] <Resin composition> The resin composition of the present invention contains at least the above-mentioned polyolefin resin (A), the acid-modified polyolefin resin (B), the tackifier (C) and the filler (D), and may further contain various additives such as an antioxidant as required.

[0027] It is desirable that the melt viscosity of the resin composition of the present invention at 230°C is 5 to 1000 dPa·s. The melt viscosity of the resin composition can be achieved by appropriately adjusting the types and mixing ratios of the polyolefin resin (A), the acid-modified polyolefin resin (B), the tackifier (C) and the filler (D). In addition, the melt viscosity at 230°C herein is a value measured as follows. That is, the resin composition is dried to a moisture content of less than 0.1%, and then the resin composition heated and stabilized at 230°C is subjected to a flow tester (model CFT-500C) manufactured by Shimadzu Corporation to flow at 98 N / cm 2 The measured value of the viscosity when passing through a 10 mm thick die with a 1.0 mm pore diameter under a pressure of . When the melt viscosity is high above 1000 dPa·s, high resin cohesion and durability can be obtained, but since high-pressure injection molding is required when sealing parts of complex shapes, part damage sometimes occurs. By using a resin composition with a melt viscosity of less than 1000 dPa·s, preferably less than 900 dPa·s, a product with excellent electrical insulation can be obtained under a relatively low injection pressure of 0.1 to 20 MPa, while the characteristics are not impaired. In addition, from the viewpoint of the operation of injecting the resin composition, the melt viscosity at 230°C is preferably low, but considering the adhesion and cohesion of the resin composition, the lower limit is preferably 5 dPa·s or more, more preferably 10 dPa·s or more, further preferably 30 dPa·s or more, and most preferably 50 dPa·s or more.

[0028] The resin composition of the present invention may further contain an antioxidant. As the antioxidant used in the present invention, there is no particular limitation as long as it is a substance that can prevent the oxidation of the polyolefin resin (A), and hindered phenol-based antioxidants, phosphorus-based antioxidants, thioether-based antioxidants, etc. can be used. For example, as hindered phenols, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,1,3-tris(4-hydroxy-2-methyl-5-tert-butylphenyl)butane, 1,1-bis(3-tert-butyl-6-methyl-4-hydroxyphenyl)butane, 3,5-bis(1,1-dimethylethyl)-4-hydroxy-phenylpropionic acid, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 3-(1,1-dimethylethyl)-4-hydroxy-5-methyl-phenylpropionic acid, 3,9 -bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyl]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-trimethyl-2,4,6-trimethyl(3',5'-di-tert-butyl-4'-hydroxybenzyl)benzene; as phosphorus-based, 3,9-bis(p-nonylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa- 3,9-diphosphaspiro[5.5]undecane, tris(monononylphenyl)phosphite, triphenoxyphosphine, isodecyl phosphite, isodecylphenyl phosphite, diphenyl 2-ethylhexyl phosphite, dinonylphenyl bis(nonylphenyl)phosphite, 1,1,3-tris(2-methyl-4-di(tridecyl)phosphite-5-tert-butylphenyl)butane, tris(2,4-di-tert-butylphenyl)phosphite, pentaerythritol bis(2,4-di-tert-butylphenyl phosphite), 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphite )-2-methylhexyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite; as thioether series, 4,4'-thiobis[2-tert-butyl-5-methylphenyl]bis[3-(dodecylthio)propionate], thiobis[2-(1,1-dimethylethyl)-5-methyl-4,1-phenylene]bis[3-(tetradecylthio)-propionate], pentaerythritol tetrakis(3-n-dodecylthiopropionate), bis(tridecyl)thiopropionate can be mentioned, and these can be used alone or in combination.

[0029] The content of the antioxidant is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and further preferably 0.3 parts by mass or more, relative to 100 parts by mass of the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B) and the tackifier (C). When the content is too little, it may have an adverse effect on the long-term durability at high temperatures. In addition, it is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and further preferably 1 part by mass or less. When the content is too much, it may have an adverse effect on adhesion, flame retardancy, etc.

[0030] In the resin composition of the present invention, it is entirely possible to mix other resins such as polyamide, polycarbonate, acrylic acid, ethylene-vinyl acetate, etc., curing agents such as isocyanate compounds, melamine, pigments such as carbon black, titanium oxide, flame retardants such as antimony trioxide, brominated polystyrene, etc., which do not belong to any of polyolefin resin (A), acid-modified polyolefin resin (B), tackifier (C) and filler (D), without damaging the effect of the present invention. By mixing these components, adhesion, flexibility, durability, etc. are sometimes improved. At this time, polyolefin resin (A) preferably contains 20 to 50% by mass, more preferably 30 to 50% by mass, relative to the entire resin composition of the present invention. When the content of polyolefin resin (A) is too little, the excellent water vapor barrier and durability of polyolefin resin (A) itself tend to decrease, and when it is too much, flexibility and adhesion tend to decrease.

[0031] Furthermore, when the resin composition of the present invention needs to have weather resistance, it is preferred to add a light stabilizer. Examples of the light stabilizer include benzotriazole-based light stabilizers, benzophenone-based light stabilizers, hindered amine-based light stabilizers, nickel-based light stabilizers, and benzoate-based light stabilizers. Examples of the benzotriazole-based light stabilizer include 2-(3,5-di-tert-amyl-2-hydroxyphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(2'-hydroxy-5'-methylphenyl)-benzotriazole, 2,4-di-tert-butyl-6-(5-chlorobenzotriazol-2-yl)phenol, and 2-[2-hydroxy-3,5-di(1,1-dimethylbenzyl)]-2H-benzotriazole. Examples of the benzophenone-based light stabilizer include 2-hydroxy-4-(octyloxy)benzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-benzophenone, 2-hydroxy-4-methoxy-benzophenone-5-sulfonic acid, 2-hydroxy-4-n-dodecyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone. Examples of hindered amine light stabilizers include bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl- [4-piperidinyl)imino}hexamethylene(2,2,6,6-tetramethyl-4-piperidinyl)imine], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-s-triazine-2,4,6(1H,3H,5H)trione, tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-s-triazine-2,4,6(1H,3H,5H)trione, etc. Examples of nickel-based light stabilizers include [2,2'-thio-bis(4-tert-octylphenol)]-2-ethylhexylamine-nickel(II), nickel dibutyldithiocarbamate, and [2',2'-thio-bis(4-tert-octylphenol)]n-butylamine-nickel. As benzoate-based light stabilizers, 2,4-di-tert-butylphenyl-3,5'-di-tert-butyl-4'-hydroxybenzoate and the like can be cited. These light stabilizers can be used alone or in combination. When added, the amount added is preferably 0.1% by mass or more and 5% by mass or less relative to the entire resin composition. When less than 0.1% by mass, the weather resistance effect may sometimes be lacking. When greater than 5% by mass, it may sometimes have an adverse effect on adhesion and the like.

[0032] <Hot Melt Adhesive Composition> The resin composition of the present invention can be used as a hot melt adhesive composition. As a hot melt adhesive composition, it can be preferably used as a sealant for electrical and electronic components. As a specific example of the method of use, by injecting the resin composition of the present invention into a mold equipped with a product to be waterproofed, a molded body in which the above-mentioned product is sealed can be obtained. More specifically, when using a screw-type hot melt molding applicator, the resin composition of the present invention can be heated and melted at about 180 to 250° C., injected into the mold through an injection nozzle, and then after a certain cooling time, the molded product is taken out from the mold to obtain a molded product.

[0033] The type of the hot melt molding applicator is not particularly limited, and examples thereof include a vertical extruder IMC-18F9 manufactured by Imoto Manufacturing Co., Ltd. and a hybrid compact vertical injection molding machine STX20 manufactured by Nissei Plastic Industries, Ltd.

[0034] This application claims the right of priority based on Japanese Patent Application No. 2022-093160 filed on June 8, 2022. The entire contents of the specification of Japanese Patent Application No. 2022-093160 filed on June 8, 2022 are cited as a reference in this application. [Example]

[0035] In order to further explain the present invention in detail, Examples and Comparative Examples are given below, but the present invention is not limited to the Examples. In addition, each measured value described in the Examples and Comparative Examples is a value measured by the following method.

[0036] <Determination of Melting Point and Glass Transition Temperature> Using a differential scanning calorimeter "DSC220" manufactured by Seiko Instruments, 5 mg of the sample was placed in an aluminum dish, covered and sealed, and heated to 230°C at a heating rate of 20°C / min to melt. Then, using liquid nitrogen, it was cooled to -130°C at a rate of 20°C / min, kept for 5 minutes, and then measured from -130°C to 230°C at a heating rate of 20°C / min. For the obtained curve, Figure 1 In the portion showing an inflection point in the DSC as shown, the intersection of the tangent line (1) obtained from the baseline before the inflection point and the tangent line (2) obtained from the baseline after the inflection point is set as the glass transition temperature (Tg), and the minimum point of the endothermic peak (× mark in the figure) is set as the melting point (Tm).

[0037] <Melting Characteristics> Using a flow tester (CFT-500C model) manufactured by Shimadzu Corporation, a resin composition dried to a moisture content of 0.1% or less was filled into a cylinder in the center of a heating body set at 230°C. After 1 minute of filling, a load of 98 N / cm was applied to the sample by a plunger. 2 The melted sample was extruded through the die (hole diameter: 1.0 mm, thickness: 10 mm) at the bottom of the cylinder at a pressure of 1.0 mm, and the plunger's descending distance and descending time were recorded to calculate the melt viscosity at 230° C. The melting characteristics (fluidity) were evaluated based on the melt viscosity value according to the following evaluation criteria. Evaluation criteria 0: Melt viscosity 5 dPa·s or more and less than 800 dPa·s △: Melt viscosity 800 dPa·s or more and less than 1000 dPa·s ×: Melt viscosity 1000 dPa·s or more

[0038] <Water vapor barrier properties> A resin composition film having a thickness of about 120 μm was produced by heat pressing using a heat press machine (SA-303 manufactured by TEST Sangyo Co., Ltd.). The hot pressing conditions were set to a temperature of 200°C, a press pressure of 10 MPa, and a press time of 30 seconds. A test piece based on JIS Z 0208: 1976 was cut from the hot pressed film using a shearing machine. The film was then mounted on a fixture specified in JIS Z 0208: 1976 and left to stand for a total of 96 hours in an environment of 25°C and 90% relative humidity (RH). The samples were taken out 24 hours, 48 ​​hours, 72 hours and 96 hours after the start of the test, and the mass was measured. The moisture permeability (water vapor barrier property) was calculated from the mass of water absorbed by calcium chloride between 24 hours and 48 hours, between 48 hours and 72 hours, and between 72 hours and 96 hours, and the average of the three moisture permeability values ​​was set as the moisture permeability. The moisture permeability was calculated according to the following formula. Moisture permeability (g / (m 2 ·24h))=(240×m) / (t×s) m: the sum of the added mass between the last two weighings of the test (mg) t: The sum of the time between the last two weighings of the test (h) s: moisture permeability area (cm 2 ) Evaluation criteria 0: Moisture permeability less than 1.0 (g / (m 2 ·24h)) △: moisture permeability 1.0(g / (m 224h)) or more, less than 1.5 (g / (m 2 ·24h)) ×: moisture permeability 1.5(g / (m 2 ·24h)) or above

[0039] <Adhesion Test (Shear Adhesion Strength)> Method for making shear bond strength test piece The substrate (aluminum substrate: A5052 (thickness: 0.5mm)) was cut into sizes of 70mm×25mm and 40mm×25mm, and the surface was wiped with acetone to remove oil. Then, the substrates were overlapped with each other by 10mm in a manner that the aluminum surface of the substrate was in contact with the molten resin composition, and the width was 25mm and the thickness of the formed resin composition was 1mm, and they were fixed inside the mold for the shear adhesion test. Then, a screw-type hot melt molding applicator (vertical low-pressure extrusion molding machine IMC-18F9 manufactured by Imoto Manufacturing Co., Ltd.) was used to inject a resin composition with a moisture content of less than 0.1% and mold it. The molding conditions were set as follows: molding resin temperature 240°C, molding pressure 4.0MPa, holding pressure 4.0MPa, holding time 20 seconds, and the ejection rotation was set to 80% (maximum ejection was set to 100%). The molded product was taken out from the mold to obtain a shear adhesion strength test piece (substrate / resin composition layer / substrate) in which the molded resin composition was sandwiched by each substrate.

[0040] Shear bond strength test method The shear bond strength test piece was stored in an atmosphere of 23°C and 50% relative humidity for 24 hours. Then, using Autograph (AG-IS manufactured by Shimadzu Corporation), each substrate was clamped with a chuck, and the resin composition layer was peeled off in the shear direction to measure the shear bond strength. The tensile speed was set to 50 mm / min. Evaluation criteria 0: Shear bond strength 2.0 MPa or more △: Shear bond strength 1.0 MPa or more and less than 2.0 MPa ×: Shear bond strength is less than 1.0 MPa

[0041] <Examples 1 to 11, Comparative Examples 1 to 5> Resin compositions (S-1) to (S-16) were obtained by melt-kneading polyolefin resin (A), acid-modified polyolefin resin (B), tackifier (C) and filler (D) at a die temperature of 160°C to 220°C using a twin-screw extruder in the proportions described in Table 1. The melting characteristics, water vapor barrier properties and shear bond strength of the resin compositions were evaluated by methods described separately. The evaluation results are shown in Table 1 below.

[0042]

Table 1

[0043] The polyolefin resin, acid-modified polyolefin resin, tackifier, and filler used in Table 1 are as follows. Polyolefin resin (A-1): J107G, manufactured by Prime Polymer Co., Ltd., homopolymer polypropylene resin, melting point: 165°C, density: 0.90 g / cm 3 Polyolefin resin (A-2): EUL731, manufactured by Sumitomo Chemical Co., Ltd., ethylene-α-olefin copolymer, melting point: 113-117°C, density: 0.90 g / cm 3 Polyolefin resin (A-3): TAFMER PN-20300, manufactured by Mitsui Chemicals, Inc., propylene-α-olefin copolymer, melting point: 160°C, density: 0.87 g / cm 3 Acid-modified polyolefin resin (B-1): PMAH1100P, manufactured by Toyobo Co., Ltd., acid-modified polypropylene resin, melting point: 147°C, molecular weight Mw: 74000 Acid-modified polyolefin resin (B-2): PMAF2, manufactured by Toyobo Co., Ltd., acid-modified polypropylene resin, melting point: 120°C, molecular weight Mw: 70,000 Thickener (C-1): YS POLYSTAR T160, manufactured by Yasuhara Chemical Co., Ltd., terpene-modified phenolic resin, hydroxyl value: 60 KOHmg / g Thickener (C-2): YS POLYSTAR G150, manufactured by Yasuhara Chemical Co., Ltd., terpene-modified phenolic resin, hydroxyl value: 140 KOHmg / g Filler (D-1): K-1, manufactured by Nippon Talc Co., Ltd., talc, plate-shaped, particle size (D50): 8.0 μm Filler (D-2): I.44P, manufactured by Volclay Japan Co., Ltd., montmorillonite, plate-shaped, size: 14-18 μm Filler (D-3): BYK-MAX CT 4255, manufactured by BYK-CHEMIE JAPAN Co., Ltd., montmorillonite, plate-shaped, particle size (D50): less than 40 μm Filler (D-4): UBS-0005E, manufactured by UNITIKA Corporation, glass beads, spherical, particle size: 5 μm or less

[0044] As can be seen from Table 1, the resin compositions of Examples 1 to 11 have excellent results in terms of water vapor barrier properties, shear adhesion strength, and melting properties. On the other hand, in Comparative Example 1, since no filler is contained, the water vapor barrier properties are poor. In Comparative Example 2, the filler content is high and there is no adhesion. In Comparative Example 3, there is less tackifier, the melt viscosity increases, and the adhesion is poor. In Comparative Example 4, due to the excessive amount of tackifier, in addition to the reduced adhesion, the water vapor barrier properties are also reduced. In Comparative Example 5, since no spherical filler is contained, the water vapor barrier properties are reduced.

Industrial Applicability

[0045] The resin composition of the present invention has a low melt viscosity during product molding, excellent adhesion to an aluminum substrate, and excellent water vapor barrier properties, and is therefore useful as a hot melt adhesive composition for waterproofing purposes.

Claims

1. A resin composition, characterized in that The invention contains a polyolefin resin (A), an acid-modified polyolefin resin (B), a tackifier (C) and a filler (D). When the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B) and the tackifier (C) is 100 parts by mass, the content of the tackifier (C) is 10 to 50 parts by mass, the content of the filler (D) is 1 to 13 parts by mass, and the filler (D) is in a plate-like shape.

2. The resin composition according to claim 1, wherein The polyolefin resin (A) includes a polypropylene resin, and further includes at least one of an ethylene-α-olefin copolymer and a propylene-α-olefin copolymer.

3. The resin composition according to claim 1 or 2, wherein The acid-modified polyolefin resin (B) has a melting point of 100° C. or higher.

4. The resin composition according to claim 1 or 2, wherein The hydroxyl value of the thickener (C) is 1 to 100 KOHmg / g.

5. The resin composition according to claim 1 or 2, wherein When the total amount of the polyolefin resin (A), the acid-modified polyolefin resin (B) and the tackifier (C) is 100 parts by mass, the content of the polyolefin resin (A) is 49 to 70 parts by mass, and the content of the acid-modified polyolefin resin (B) is 1 to 30 parts by mass. 6 . A hot melt adhesive composition comprising the resin composition according to claim 1 or 2 .