Treatment agent for short fibers, treatment agent set for short fibers, composition containing treatment agent for short fibers, first treatment agent for short fibers, second treatment agent for short fibers, composition containing first treatment agent for short fibers, composition containing second treatment agent for short fibers, synthetic fibers, and method for producing non-woven fabric
By rationally formulating alkyl phosphate salts, paraffin and polyoxyalkylene polyol fatty acid esters in the treatment agent for short fibers, the problem of insufficient antistatic and stability in the prior art has been solved, and more efficient Water repellency and antistatic properties inhibit the generation of scum.
Patent Information
- Application Number
- CN202380029608.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-23
AI Technical Summary
The existing treatment agent for short fibers has problems of insufficient antistatic and stability in improving carding processability and suppressing scum.
Use a treatment agent for short fiber containing alkyl phosphate salts, paraffin and polyoxyalkylene polyol fatty acid esters to ensure that the content of alkyl phosphate salts in its non-volatile components is more than 5% or less, and paraffin is The content is 30% or less than 75%, the content of the polyoxyalkylene polyol fatty acid ester is 2% or less than 15%, and it may contain a nonionic surfactant to form an appropriate combination to improve the stability of the treatment agent and Water-relieving nature.
The antistatic and water-repellent properties of the treatment agent for staple fiber are significantly improved, the stability of the treatment agent is enhanced, especially in low humidity, showing good antistatic properties, and suppressing the generation of scum.
Smart Images

Figure BDA0005055074390000201 
Figure BDA0005055074390000251 
Figure BDA0005055074390000261
Abstract
Description
Technical Field
[0001] The present invention relates to a processing agent for staple fibers, a processing agent kit for staple fibers, a composition containing the processing agent for staple fibers, a first processing agent for staple fibers, a second processing agent for staple fibers, a composition containing the first processing agent for staple fibers, a composition containing the second processing agent for staple fibers, synthetic fibers, and a method for producing nonwoven fabrics. Background Art
[0002] Generally, synthetic fibers are used as raw materials for nonwoven fabrics. For example, after short fibers (staple) are produced from synthetic fibers, the short fibers are passed through a carding machine to produce a carded web, thereby forming a nonwoven fabric. In addition, by applying a treatment agent for short fibers to synthetic fibers, functions such as water repellency are imparted. Nonwoven fabrics made from synthetic fibers with functions such as water repellency are used in a wide range of fields such as the health care field, the medical field, and the civil engineering field.
[0003] At present, there are known processing agents for staple fibers disclosed in Patent Documents 1 and 2. Patent Document 1 discloses a processing agent for staple fibers, which contains a specific ratio of component (A) an alkyl phosphate having a hydrocarbon group with 14 to 22 carbon atoms, etc., component (B) an ester compound formed by an alcohol having a hydrocarbon group with 6 to 22 carbon atoms and a fatty acid having a hydrocarbon group with 6 to 22 carbon atoms, and component (C) a polysilicone compound. Patent Document 2 discloses a processing agent for staple fibers, which contains a specific ratio of component (A) an ester compound formed by a monohydric alcohol having a hydrocarbon group with 12 to 22 carbon atoms and a monohydric fatty acid having a hydrocarbon group with 12 to 22 carbon atoms, component (B) an alkyl phosphate ester salt having an alkyl group with 4 to 8 carbon atoms, etc., and component (C) a fatty acid having a hydrocarbon group with 12 to 22 carbon atoms, etc. Prior art literature Patent Literature
[0004] Patent Document 1: International Publication No. 2017 / 199702 Patent Document 2: Japanese Patent No. 6906822 Summary of the invention Problems to be solved by the invention
[0005] However, in addition to imparting water repellency and other functions to the staple fibers, the staple fiber treatment agent is also expected to improve the combing processability in the manufacturing process of nonwoven fabrics and suppress the scum generated in the production line in the staple fiber manufacturing process. In order to improve the combing processability, it is necessary to improve the antistatic property of the synthetic fiber to which the staple fiber treatment agent is attached. In addition, in order to suppress scum, it is necessary to improve the stability of the staple fiber treatment agent, for example. Means for solving problems
[0006] The present inventors have conducted studies to solve the above-mentioned problems and have found that a composition comprising a specific alkyl phosphate salt, a paraffin wax, and a polyoxyalkylene polyol fatty acid ester is particularly effective.
[0007] In order to solve the above-mentioned problems, one form of the short fiber processing agent of the present invention focuses on: containing the later-mentioned component (A), the later-mentioned component (B), and the later-mentioned component (C), and the non-volatile component of the short fiber processing agent contains 5 mass% to 50 mass% of the above-mentioned component (A), 30 mass% to 75 mass% of the above-mentioned component (B), and 2 mass% to 15 mass% of the above-mentioned component (C).
[0008] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester.
[0009] The short fiber processing agent may contain 40% to 70% by mass of the component (B) and 2% to 10% by mass of the component (C) in the nonvolatile content.
[0010] The short fiber processing agent may further contain a component (D) described later. Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C).
[0011] The nonvolatile content of the short fiber processing agent may contain 2% by mass or more and 10% by mass or less of the component (D). The non-volatile component of the above-mentioned short fiber processing agent may also contain the above-mentioned component (A) at least 20 mass % and less than 40 mass %, the above-mentioned component (B) at least 45 mass % and less than 65 mass %, the above-mentioned component (C) at least 4 mass % and less than 8 mass %, and the above-mentioned component (D) at least 4 mass % and less than 8 mass %.
[0012] In order to solve the above-mentioned problems, a staple fiber treatment agent kit of one form of the present invention focuses on: it includes a first staple fiber treatment agent and a second staple fiber treatment agent in a group, the first staple fiber treatment agent contains the component (B) described later, the component (C) described later, and arbitrarily and selectively contains the component (D) described later, the second staple fiber treatment agent contains the component (A) described later, and when the first staple fiber treatment agent and the second staple fiber treatment agent are mixed, the non-volatile component of the obtained staple fiber treatment agent contains 5 mass % to 50 mass % of the component (A), 30 mass % to 75 mass % of the component (B), and 2 mass % to 15 mass % of the component (C).
[0013] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester.
[0014] Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C). In order to solve the above-mentioned problems, a composition containing a short fiber processing agent according to one aspect of the present invention mainly contains the short fiber processing agent and a solvent.
[0015] In order to solve the above-mentioned problems, a composition containing a short fiber treatment agent according to one aspect of the present invention mainly contains the first short fiber treatment agent, the second short fiber treatment agent, and a solvent in the short fiber treatment agent set.
[0016] In order to solve the above-mentioned problems, the first treatment agent for staple fibers of one form of the present invention focuses on the following aspects: when in use, it is used together with the second treatment agent for staple fibers containing the component (A) described later; when not in use, it is constituted in a different agent form from the second treatment agent for staple fibers, contains the component (B) described later, the component (C) described later, and optionally contains the component (D) described later; when the first treatment agent for staple fibers and the second treatment agent for staple fibers are mixed, the non-volatile component of the obtained treatment agent for staple fibers contains 5% by mass to 50% by mass of the component (A), 30% by mass to 75% by mass of the component (B), and 2% by mass to 15% by mass of the component (C).
[0017] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester.
[0018] Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C). In order to solve the above-mentioned problems, the second treatment agent for staple fibers of one form of the present invention focuses on the following aspects: when in use, it is used in combination with the first treatment agent for staple fibers containing the component (B) described later, the component (C) described later, and optionally containing the component (D) described later; when not in use, it is constituted in a different agent form from the first treatment agent for staple fibers, containing the component (A) described later; when the first treatment agent for staple fibers and the second treatment agent for staple fibers are mixed, the non-volatile component of the obtained treatment agent for staple fibers contains 5% by mass to 50% by mass of the component (A), 30% by mass to 75% by mass of the component (B), and 2% by mass to 15% by mass of the component (C).
[0019] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester. Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C).
[0020] In order to solve the above-mentioned problems, a composition containing a first treatment agent for short fibers according to one aspect of the present invention mainly contains the above-mentioned first treatment agent for short fibers and a solvent.
[0021] In order to solve the above-mentioned problems, a composition containing a second treatment agent for short fibers according to one aspect of the present invention mainly contains the above-mentioned second treatment agent for short fibers and a solvent. In order to solve the above-mentioned problems, a synthetic fiber according to one aspect of the present invention mainly has the above-mentioned short fiber treating agent attached thereto.
[0022] In order to solve the above problems, a synthetic fiber according to one aspect of the present invention mainly has a staple fiber treatment agent attached thereto, which is a mixture of the first staple fiber treatment agent and the second staple fiber treatment agent in the staple fiber treatment agent set.
[0023] In order to solve the above-mentioned problems, a method for producing a nonwoven fabric according to one aspect of the present invention mainly includes the following steps 1 to 3. Step 1: The above-mentioned short fiber treating agent is attached to the synthetic fiber.
[0024] Step 2: The synthetic fibers to which the short fiber treating agent is attached in the above step 1 are passed through a carding machine to obtain a carded web. Step 3: The carded web obtained in the above step 2 is subjected to a heat fusion treatment to obtain a nonwoven fabric.
[0025] In order to solve the above-mentioned problems, a method for producing a nonwoven fabric according to one aspect of the present invention mainly includes the following steps 1 to 3. Step 1: A short fiber treatment agent is attached to synthetic fibers. The short fiber treatment agent is a mixture of the first short fiber treatment agent and the second short fiber treatment agent in the short fiber treatment agent set.
[0026] Step 2: The synthetic fibers to which the short fiber treating agent is attached in the above step 1 are passed through a carding machine to obtain a carded web. Step 3: The carded web obtained in the above step 2 is subjected to a heat fusion treatment to obtain a nonwoven fabric.
[0027] The method for producing the nonwoven fabric may be such that: the synthetic fiber is a polyolefin-based synthetic fiber. Effects of the Invention
[0028] According to the present invention, the stability of the short fiber processing agent can be improved, and the water repellency and antistatic property imparted by the short fiber processing agent to the fiber can be improved. DETAILED DESCRIPTION
[0029] <First embodiment> A first embodiment that specifically implements the short fiber processing agent (hereinafter referred to as the processing agent) according to the present invention will be described.
[0030] The treatment agent of this embodiment contains an alkyl phosphate having an alkyl group with 1 to 5 carbon atoms as component (A), a paraffin as component (B), and a polyoxyalkylene polyol fatty acid ester as component (C). The treatment agent may further contain a nonionic surfactant having a (poly)oxyalkylene structure in the molecule as component (D), which is different from component (C).
[0031] (Ingredient (A): alkyl phosphate) The component (A) used in the treatment agent of the present embodiment is an alkyl phosphate having an alkyl group with a carbon number of 1 to 5. By including the component (A) in the treatment agent, the antistatic property imparted by the treatment agent to the fiber can be improved.
[0032] The alkyl group constituting the alkyl phosphate salt may be a straight chain or a branched chain. The alkyl phosphate salt includes, for example, a single monoester, a single diester, a mixture of a monoester and a diester, etc. The diester may be a symmetrical diester having the same alkyl group or an asymmetrical diester having different alkyl groups. In addition, it may also be a diphosphate.
[0033] The number of carbon atoms in the alkyl group is 1 to 5, preferably 2 to 4. Specific examples of the alkyl group include methyl, ethyl, propyl, butyl, pentyl, isobutyl, and isopentyl.
[0034] The phosphoric acid constituting the alkyl phosphate salt is not particularly limited, and may be orthophosphoric acid or polyphosphoric acid such as diphosphoric acid. Examples of the salt constituting the alkyl phosphate salt include phosphate metal salts, phosphate amine salts, and phosphate ammonium salts.
[0035] Examples of metal salts include alkali metal salts and alkaline earth metal salts. Specific examples of alkali metals constituting alkali metal salts include sodium, potassium, lithium, etc. Alkaline earth metals constituting alkaline earth metal salts include members of Group 2 elements, such as calcium, magnesium, beryllium, strontium, barium, etc. Among these salts, alkali metal salts are preferred, and potassium salts are more preferred.
[0036] The amine constituting the amine salt may be any of a primary amine, a secondary amine, and a tertiary amine. Examples of the amines constituting the amine salts include (1) aliphatic amines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, NN-diisopropylethylamine, butylamine, dibutylamine, 2-methylbutylamine, tributylamine, octylamine, and dimethyllaurylamine; (2) aromatic amines or heterocyclic amines such as aniline, N-methylbenzylamine, pyridine, morpholine, piperazine, and derivatives thereof; (3) alkanolamines such as monoethanolamine, N-methylethanolamine, diethanolamine, triethanolamine, isopropanolamine, diisopropanolamine, triisopropanolamine, dibutylethanolamine, butyldiethanolamine, octyldiethanolamine, and lauryldiethanolamine; (4) arylamines such as N-methylbenzylamine; (5) polyoxyalkylene alkylamine ethers such as polyoxyethylene laurylamine ether and polyoxyethylene stearylamine ether; (6) ammonia, etc.
[0037] Among these, salts of alkyl phosphates having an alkyl group having 2 to 4 carbon atoms are preferred because the effects of the present invention are excellent.
[0038] Specific examples of the component (A) include potassium salts of ethyl phosphate, potassium salts of propyl phosphate, potassium salts of butyl phosphate, diethanolamine salts of propyl phosphate, and diethanolamine salts of butyl phosphate. These components (A) may be used alone or in combination of two or more. The lower limit of the content ratio of component (A) in the non-volatile components of the treatment agent can be appropriately set, preferably 5% by mass or more, more preferably 7.5% by mass or more. When the content ratio is 5% by mass or more, the antistatic property imparted by the treatment agent to the fiber can be further improved. The upper limit of the content ratio of the component (A) can be appropriately set, preferably 50% by mass or less, more preferably 45% by mass or less. When the content ratio is 50% by mass or less, the water repellency imparted by the treatment agent to the fiber can be further improved. Among them, it can also be a range of any combination of the above upper and lower limits. In this specification, the non-volatile component refers to the residue after the object is heat-treated at 105°C for 2 hours to fully remove the volatile substances, that is, the absolutely dry product.
[0039] In addition, when the treatment agent contains the component (D) described later, the lower limit of the content ratio of the component (A) in the non-volatile component of the treatment agent can be appropriately set, preferably 5% by mass or more, more preferably 20% by mass or more. When the content ratio is 5% by mass or more, the antistatic property of the treatment agent on the fiber can be further improved. The upper limit of the content ratio of the component (A) can be appropriately set, preferably 50% by mass or less, more preferably 40% by mass or less. When the content ratio is 50% by mass or less, the water repellency of the treatment agent on the fiber can be further improved. Among them, it can also be the range of any combination of the above upper and lower limits.
[0040] (Ingredient (B): paraffin) The component (B) used in the treatment agent of the present embodiment is paraffin wax. By including the component (B) in the treatment agent, the water repellency imparted by the treatment agent to the fiber can be improved.
[0041] The paraffin wax is not particularly limited as long as it is a hydrocarbon that can be used as a treatment agent. The paraffin wax may be a commercial product with a defined melting point. The melting point may be appropriately set, preferably 50°C to 70°C, more preferably 50°C to 60°C. It may also be a range of any combination of the upper and lower limits mentioned above.
[0042] The lower limit of the content of component (B) in the non-volatile component of the treatment agent can be appropriately set, preferably 30% by mass or more, more preferably 40% by mass or more. When the content is 30% by mass or more, the water repellency of the treatment agent to the fiber can be further improved. The upper limit of the content of component (B) can be appropriately set, preferably 75% by mass or less, more preferably 70% by mass or less. When the content is 75% by mass or less, the stability of the treatment agent can be further improved. Among them, it can also be a range of any combination of the above upper and lower limits.
[0043] In addition, when the treatment agent contains the component (D) described later, the lower limit of the content ratio of the component (B) in the non-volatile component of the treatment agent can be appropriately set, preferably 30% by mass or more, more preferably 45% by mass or more. When the content ratio is 30% by mass or more, the water repellency given by the treatment agent to the fiber can be further improved. The upper limit of the content ratio of the component (B) can be appropriately set, preferably 75% by mass or less, more preferably 65% by mass or less. When the content ratio is 75% by mass or less, the stability of the treatment agent can be further improved. Among them, it can also be a range of any combination of the above upper and lower limits.
[0044] (Component (C): polyoxyalkylene polyol fatty acid ester) The component (C) used in the treatment agent of the present embodiment is a polyoxyalkylene polyol fatty acid ester. By including the component (C) in the treatment agent, the stability of the treatment agent can be improved.
[0045] Specific examples of carboxylic acids used as raw materials for component (C) include, for example, (1) straight-chain alkyl carboxylic acids such as octanoic acid, nonanoic acid, decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid, heptadecanoic acid, octadecanoic acid, nonadecanoic acid, eicosanoic acid, heneicosanoic acid, and docosanoic acid; (2) branched-chain alkyl carboxylic acids such as 2-ethylhexanoic acid, isododecanoic acid, isotridecanoic acid, isotetradecanoic acid, isohexadecanoic acid, and isooctadecanoic acid; (3) straight-chain alkenyl carboxylic acids such as octadecenoic acid, octadecadienoic acid, and octadecatrienoic acid; and (4) hydroxycarboxylic acids such as ricinoleic acid.
[0046] The alkylene oxide used as the raw material for forming the polyoxyalkylene structure in component (C) is preferably an alkylene oxide having a carbon number of 2 or more and 4 or less. Specific examples of alkylene oxides include ethylene oxide, propylene oxide, butylene oxide, etc. The number of moles of alkylene oxide added can be appropriately set, preferably 0.1 mole or more and 60 moles or less, more preferably 1 mole or more and 40 moles or less, and most preferably 2 moles or more and 30 moles or less. It can also be a range of any combination of the above upper and lower limits. Among them, the number of moles of alkylene oxide added represents the number of moles of alkylene oxide relative to 1 mole of the addition object compound in the loading raw material. Alkylene oxide can use one type of alkylene oxide alone, or two or more alkylene oxides can be used in appropriate combination. When two or more types of alkylene oxides are used, these addition forms can be any one of block addition, random addition, and a combination of block addition and random addition, without special restrictions.
[0047] Specific examples of the polyol used as a raw material for the component (C) include ethylene glycol, propylene glycol, 1,3-propane diol, 1,2-butane diol, 1,3-butane diol, 1,4-butane diol, 2-methyl-1,2-propane diol, 1,5-pentane diol, 1,6-hexane diol, 2,5-hexane diol, 2-methyl-2,4-pentane diol, 2,3-dimethyl-2,3-butane diol, glycerol, 2-methyl-2-hydroxymethyl-1,3-propane diol, trimethylolpropane, sorbitan, pentaerythritol, sorbitol, and the like.
[0048] Among these, polyoxyalkylene sorbitan fatty acid esters are preferred because the effects of the present invention can be further enhanced. Specific examples of component (C) include polyoxyethylene (10: represents the number of added moles of alkylene oxide (the same applies hereinafter)) sorbitan monooleyl ester, polyoxyethylene (20) sorbitan monooctadecyl ester, polyoxyethylene (10) glycerol monooleyl ester, polyoxyethylene (20) glycerol monooctadecyl ester, polyoxyethylene (10) 1,6-hexanediol dilauryl ester, and polyoxyethylene (10) trimethylolpropane trilauryl ester.
[0049] These components (C) may be used alone or in combination of two or more. The lower limit of the content ratio of component (C) in the non-volatile component of the treatment agent can be appropriately set, preferably 1% by mass or more, more preferably 2% by mass or more. When the content ratio is 1% by mass or more, the stability of the treatment agent can be further improved. The upper limit of the content ratio of the component (C) can be appropriately set, preferably 15% by mass or less, more preferably 10% by mass or less. When the content ratio is 15% by mass or less, the effect of the present invention can be further improved. Wherein, it can also be the range of any combination of the above upper and lower limits.
[0050] In addition, when the treatment agent contains the component (D) described later, the lower limit of the content ratio of the component (C) in the non-volatile component of the treatment agent can be appropriately set, preferably 1% by mass or more, more preferably 4% by mass or more. When the content ratio is 1% by mass or more, the stability of the treatment agent can be further improved. The upper limit of the content ratio of the component (C) can be appropriately set, preferably 15% by mass or less, more preferably 8% by mass or less. When the content ratio is 15% by mass or less, the effect of the present invention can be further improved. Wherein, it can also be the range of any combination of the above upper and lower limits.
[0051] (Ingredient (D): nonionic surfactant) From the viewpoint of further improving the stability of the treatment agent, the treatment agent may further contain a component (D). The component (D) used in the treatment agent of this embodiment is a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to the above-mentioned component (C).
[0052] Examples of the component (D) include those having a (poly)oxyalkylene structure obtained by adding alkylene oxide to alcohols or carboxylic acids, and those having a (poly)oxyalkylene structure obtained by adding alkylene oxide to alkylamines as amine compounds.
[0053] Specific examples of alcohols used as a raw material for component (D) include, for example, (1) straight-chain alkanols such as methanol, ethanol, propanol, butanol, pentanol, hexanol, octanol, nonanol, decanol, undecanol, dodecanol, tridecanol, tetradecanol, pentadecanol, hexadecanol, heptadecanol, octadecanol, nonadecanol, eicosanol, heneicosanol, docosanol, tricosanol, tetracosanol, pentacosanol, hexacosanol, heptacosanol, octacosanol, nonacosanol, and triacontanol; (2) isopropyl alcohol, isobutyl alcohol, isohexanol, 2-ethylhexanol, isononanol, isodecanol, isotridecanol, isotetradecanol, isobutyl alcohol, isobutyl alcohol, isohexanol, 2-ethylhexanol, isononanol, isodecanol, isododecanol, isotridecanol, isotetradecanol, isobutyl alcohol ... (i) branched alkanols such as pentadecanol, isohexadecanol, isoheptadecanol, isooctadecanol, isonadecanol, isoeicosanol, isoheneicosanol, isodocosanol, isotricosanol, isotetracosanol, isopentacosanol, isohexacosanol, isohexacosanol, isohexacosanol, isooctacosanol, isonoctanol, isotriacontanol, etc.; (2) straight-chain alkanols such as tetradecanol, hexadecanol, heptadecanol, octadecanol, nonadecanol, etc.; (3) branched alkanols such as tetradecanol, hexadecanol, heptadecanol, octadecanol, nonadecanol, etc.; (4) branched alkanols such as isohexadecanol and isooctadecanol; (5) cyclic alkanols such as cyclopentanol and cyclohexanol; (6) aromatic alcohols such as phenol, nonylphenol, benzyl alcohol, monostyrenated phenol, distyrenated phenol, tristyrenated phenol, etc.
[0054] Specific examples of the alkylamine used as a raw material of the component (D) include methylamine, ethylamine, butylamine, octylamine, laurylamine, octadecylamine, octadecylamine, coconut amine, and the like.
[0055] As the carboxylic acid used as the raw material of the component (D), those listed as the raw materials of the above-mentioned component (C) can be applied as the raw material for forming the (poly)oxyalkylene structure of the component (D).
[0056] Specific examples of the component (D) include polyoxyethylene (18) oleyl ether, polyoxyethylene (10) lauryl ether, polyoxyethylene (10) lauryl amino ether, polyoxyethylene (7) oleyl ester, polyoxyethylene (7) stearyl ether, and polyoxyethylene (5) oleyl ether.
[0057] These components (D) may be used alone or in combination of two or more. The lower limit of the content ratio of component (D) in the non-volatile components of the treatment agent can be appropriately set, preferably 1% by mass or more, more preferably 2% by mass or more, and optimally 4% by mass or more. When the content ratio is 1% by mass or more, the stability of the treatment agent can be further improved. The upper limit of the content ratio of the component (D) can be appropriately set, preferably 15% by mass or less, more preferably 10% by mass or less, and optimally 8% by mass or less. When the content ratio is 15% by mass or less, the water repellency imparted by the treatment agent to the fiber can be further improved. Among them, it can also be a range of any combination of the above upper and lower limits.
[0058] (Save form) The treatment agent may also be composed of a combination of a first treatment agent for staple fibers (hereinafter referred to as "the first treatment agent") and a second treatment agent for staple fibers (hereinafter referred to as "the second treatment agent"), wherein the first treatment agent contains the above-mentioned component (B), component (C), and optionally contains component (D), and the second treatment agent contains the above-mentioned component (A). In other words, the treatment agent may also be a treatment agent set for staple fibers that contains the first treatment agent and the second treatment agent in a group. The treatment agent set for staple fibers may also be a combination of the first treatment agent and the second treatment agent. Before use, such as during storage or circulation, the treatment agent is composed of the first treatment agent and the second treatment agent, wherein the second treatment agent is composed of a different agent from the first treatment agent. The treatment agent is prepared into a mixture of the first treatment agent and the second treatment agent when it is used.
[0059] (Solvent) The treatment agent of this embodiment can also be mixed with a solvent as appropriate to prepare a composition containing the treatment agent for short fibers (hereinafter referred to as a "composition containing the treatment agent"), and stored or circulated in the form of a composition containing the treatment agent. This structure can improve the homogeneity and stability of the mixture when it is further diluted with a solvent during use.
[0060] The solvent is a solvent having a boiling point of 105° C. or less at atmospheric pressure. Examples of the solvent include water and organic solvents. Specific examples of organic solvents include lower alcohols such as ethanol and propanol, or low polar solvents such as hexane. These solvents may be used alone or in combination of two or more. Among these, polar solvents such as water and lower alcohols are preferred from the perspective of excellent dispersibility or solubility of each component, and water is more preferred from the perspective of excellent operability.
[0061] When the total content of the treatment agent and the solvent in the treatment agent-containing composition is 100 parts by mass, the treatment agent is preferably contained in an amount of 10 parts by mass or more and 80 parts by mass or less. The effects of the treatment agent according to the first embodiment described above will be described.
[0062] (1-1) The treatment agent of the first embodiment contains the above-mentioned component (A), component (B), and component (C). Therefore, the stability of the treatment agent for short fibers can be improved, and the water repellency and antistatic properties imparted by the treatment agent for short fibers to the fibers can be improved. In particular, the antistatic properties under low humidity can be improved.
[0063] (1-2) When the treatment agent of the first embodiment further contains the component (D), the stability of the treatment agent can be further improved. (1-3) The treatment agent of the first embodiment may also be composed of a combination of a first treatment agent and a second treatment agent before use, such as during storage or circulation, wherein the first treatment agent contains the above-mentioned component (B), component (C), and optionally contains component (D), and the second treatment agent contains the above-mentioned component (A). With this configuration, the formulation stability, especially the storage stability, of the treatment agent before use, such as during storage or circulation, can be further improved.
[0064] <Second embodiment> Next, a second embodiment that embodies the first treatment agent according to the present invention will be described, with the description focusing on differences from the first embodiment.
[0065] The first treatment agent of this embodiment contains the above-mentioned component (B), component (C), and optionally contains component (D). When the first treatment agent is used, it is used together with the second treatment agent containing the above-mentioned component (A), and when not used, it is composed of different agents with the second treatment agent. In other words, the treatment agent is prepared into a mixture of the first treatment agent and the second treatment agent when it is used. Components (A) to (D) are the same as the components described in the first embodiment.
[0066] (Solvent) The first treatment agent of this embodiment can also be mixed with a solvent as appropriate to prepare a composition containing the first treatment agent for short fibers (hereinafter referred to as "the composition containing the first treatment agent"), and stored or circulated in the form of the composition containing the first treatment agent. This configuration can improve the miscibility when diluted with a solvent or mixed with the second treatment agent during use, and improve the stability of the composition.
[0067] The solvent may be the one exemplified in the first embodiment. When the total content of the first treatment agent and the solvent in the composition containing the first treatment agent is 100 parts by mass, the first treatment agent is preferably contained in an amount of 10 parts by mass to 80 parts by mass.
[0068] The effect of the first treatment agent of the second embodiment described above will be described. The second embodiment described above has the following effects in addition to the effects of the first embodiment. (2-1) The first treatment agent of the second embodiment contains the above-mentioned component (B), component (C), and optionally contains component (D), and when not in use, it is composed of a different agent from the second treatment agent containing the above-mentioned component (A). The first treatment agent is used together with the second treatment agent only when in use, and a mixture of the first treatment agent and the second treatment agent is prepared. Therefore, the formulation stability of the first treatment agent before use, such as during storage or circulation, in particular the storage stability, can be further improved. In addition, the composition of the obtained treatment agent can be adjusted by adjusting the mixing ratio with the second treatment agent. In addition, the first treatment agent and the second treatment agent can be circulated separately.
[0069] <Third embodiment> Next, a third embodiment that embodies the second treatment agent according to the present invention will be described, with the description focusing on differences from the first and second embodiments.
[0070] The second treatment agent of this embodiment contains the above-mentioned component (A). When the second treatment agent is used, it is used together with the first treatment agent containing the above-mentioned component (B), component (C), and optionally containing component (D). When not used, it is composed of different agents from the first treatment agent. In other words, the treatment agent is prepared into a mixture of the first treatment agent and the second treatment agent when it is used. Components (A) to (D) are the same as the components described in the first embodiment.
[0071] (Solvent) The second treatment agent of this embodiment can also be mixed with a solvent as appropriate to prepare a composition containing the second treatment agent for short fibers (hereinafter referred to as "the composition containing the second treatment agent"), and stored or circulated in the form of the composition containing the second treatment agent. This structure can improve the miscibility when diluted with a solvent or mixed with the first treatment agent during use, and improve the stability of the composition.
[0072] The solvent may be the one exemplified in the first embodiment. When the total content of the second treatment agent and the solvent in the composition containing the second treatment agent is 100 parts by mass, the second treatment agent is preferably contained in an amount of 10 parts by mass to 80 parts by mass.
[0073] The effects of the second treatment agent of the third embodiment described above will be described. The third embodiment has the following effects in addition to the effects of the first and second embodiments. (3-1) The second treatment agent of the third embodiment contains the above-mentioned component (A), and when not in use, it is constituted in a different agent form from the first treatment agent containing the above-mentioned component (B), component (C), and optionally containing component (D). The second treatment agent is used together with the first treatment agent only when in use, and a mixture of the first treatment agent and the second treatment agent is prepared. Therefore, the formulation stability of the second treatment agent before use, such as during storage or circulation, in particular the storage stability, can be further improved. In addition, the composition of the obtained treatment agent can be adjusted by adjusting the mixing ratio with the first treatment agent. In addition, the second treatment agent can be circulated separately from the first treatment agent.
[0074] <Fourth embodiment> A fourth embodiment of the synthetic fiber according to the present invention will be described. The synthetic fiber of this embodiment has the treatment agent of the first embodiment attached thereto.
[0075] (synthetic fiber) Specific examples of synthetic fibers include (1) polyolefin fibers such as polyethylene fibers, polypropylene fibers, and polybutene fibers; (2) polyester fibers such as polyethylene terephthalate, polybutylene terephthalate, polyethylene terephthalate / isophthalate, and polyether polyester; (3) polyamide fibers such as nylon 6 and nylon 66; and (4) composite fibers having a core-sheath structure (composite fibers in which either or both of the core and sheath are polyolefin fibers, such as polyethylene / polypropylene composite fibers or polyethylene / polyester composite fibers in which the sheath is polyethylene fiber, or polyethylene / polypropylene composite fibers or polyethylene / polyester composite fibers having a parallel structure). Among these, preferred are: polyolefin fibers such as polyethylene fibers, polypropylene fibers, and polybutene fibers; composite fibers having a core-sheath structure (composite fibers in which either or both of the core and sheath are polyolefin fibers, such as polyethylene / polypropylene composite fibers, polyethylene / polyester composite fibers in which the sheath is polyethylene fiber, or polyethylene / polypropylene composite fibers, polyethylene / polyester composite fibers having a parallel structure, etc.). Here, the so-called polyolefin synthetic fibers refer to synthetic fibers synthesized using olefins (alkene) as monomers.
[0076] (Uses of Fiber) The use of the fiber with the treatment agent attached thereto includes short fibers. Short fibers are generally referred to as "staples" and do not include long fibers called "filaments". In addition, the length of the short fibers is not particularly limited as long as it meets the definition of short fibers in the technical field, for example, 100 mm or less, preferably 30 mm or more and 70 mm or less.
[0077] (Attachment treatment of treatment agent) The ratio of the treatment agent of the first embodiment to be attached to the synthetic fiber is not particularly limited, but the treatment agent not containing a solvent is preferably attached at 0.1% by mass to 2% by mass, more preferably 0.3% by mass to 1.2% by mass, relative to the synthetic fiber.
[0078] The method for making the treatment agent adhere to the synthetic fiber, for example, can be applied as follows: using a composition containing the treatment agent of the first embodiment and water, or a diluent diluted with a solvent, to make it adhere by a known method, such as an immersion method, a spray method, a drum method, a guided oiling method using a metering pump, etc.
[0079] The composition or diluent containing the treatment agent can be prepared by a known mechanical emulsification method using a stirrer, a homogenizer or the like. (Method for producing nonwoven fabric) The synthetic fiber of this embodiment can also be used to produce a nonwoven fabric by the following method.
[0080] Step 1: The treatment agent of the first embodiment is allowed to adhere to synthetic fibers. Step 2: The synthetic fibers to which the treatment agent is attached in the above step 1 are passed through a carding machine to obtain a carded web.
[0081] Step 3: The carded web obtained in the above step 2 is subjected to a heat fusion treatment to obtain a nonwoven fabric. By following the above steps, nonwoven fabric can be manufactured. Since nonwoven fabric is formed by heat-fusion bonding fibers, it can also be called heat-fusion bonded nonwoven fabric.
[0082] When a nonwoven fabric is produced from short fibers, polyolefin-based synthetic fibers are preferably used as the synthetic fibers from the viewpoint of excellent productivity and usage characteristics. The temperature of the heat fusion treatment can be appropriately set depending on the type of synthetic fiber, the treatment time, etc., and can be, for example, 100° C. to 180° C., preferably 120° C. to 160° C. The time of the heat fusion treatment can be appropriately set depending on the type of synthetic fiber, the treatment temperature, etc., and can be, for example, 1 second to 60 seconds, preferably 5 seconds to 20 seconds.
[0083] The effects of the synthetic fiber of the fourth embodiment will be described. (4-1) The synthetic fiber of the fourth embodiment is attached with a treatment agent, which contains the above-mentioned component (A), component (B), and component (C). Therefore, the water repellency and antistatic property of the synthetic fiber can be improved. By improving the antistatic property, the carding processability during the manufacture of nonwoven fabrics can be improved. In addition, by improving the stability of the treatment agent, scum can be suppressed, especially in the short fiber manufacturing step. In addition, a highly safe synthetic fiber can be obtained.
[0084] (4-2) When the synthetic fiber of the fourth embodiment is used to produce a heat-fusible nonwoven fabric, the bonding of the fibers during the heat-fusion treatment is not hindered. In addition, the treatment agent is less likely to volatilize at high temperatures. The above-mentioned embodiment can also be implemented with modifications as follows: The above-mentioned embodiment and the following modifications can be implemented in combination with each other within the scope of no technical contradiction.
[0085] The method for producing the nonwoven fabric of the above-mentioned embodiment is not particularly limited, and a method other than the method for producing the nonwoven fabric described in the description of the fourth embodiment may be employed. The treatment agent or composition may also contain stabilizers or antistatic agents for maintaining the quality of the treatment agent or composition, smoothing agents other than those mentioned above, surfactants other than those mentioned above, antistatic agents, antistatic auxiliary agents such as polyols, linkers, antioxidants, ultraviolet absorbers, defoamers, and other components that are commonly used in treatment agents, within the range that does not impair the effects of the present invention. Among them, from the viewpoint of effectively exerting the effects of the present invention, other components that are commonly used in treatment agents other than the solvent are preferably 40% by mass or less, more preferably 20% by mass or less in each treatment agent. Example
[0086] In order to more specifically explain the constitution and effects of the present invention, examples are given below, but the present invention is not limited to these examples. In the following examples and comparative examples, unless otherwise specified, part represents part by mass, and % represents mass %.
[0087] Test Category 1 (Preparation of treatment agent) (Example 1) As shown in Table 1, 30 parts (%) of potassium salt of ethyl phosphate (A-1) of alkyl phosphate ester salt (A), 60 parts (%) of paraffin (B-1) with a melting point of 55°C of paraffin (B), 5 parts (%) of polyoxyethylene (10) sorbitan monooleyl ester (C-1) of polyoxyalkylene polyol fatty acid ester (C), and 5 parts (%) of polyoxyethylene (18) oleyl ether (D-1) of nonionic surfactant (D) were weighed and added to a container. These were stirred and mixed uniformly at a temperature of about 80°C. Furthermore, 150 parts of water at 20°C was added to the container while stirring and mixing uniformly, and the total amount was 250 parts. Then, emulsification was performed to prepare a composition containing 40% of the treatment agent of Example 1.
[0088] (Examples 2 to 25, Comparative Examples 1 to 11) The treatment agents of Examples 2 to 25 and Comparative Examples 1 to 11 were prepared in the same manner as the treatment agent of Example 1, and contained alkyl phosphate salts (A), paraffin (B), polyoxyalkylene polyol fatty acid esters (C), nonionic surfactants (D), and other components (E) in the proportions shown in Table 1.
[0089] The type and content of the alkyl phosphate salt (A), the type and content of the paraffin (B), the type and content of the polyoxyalkylene polyol fatty acid ester (C), the type and content of the nonionic surfactant (D), and the type and content of other components (E) are shown in the "Component (A)" column, "Component (B)" column, "Component (C)" column, "Component (D)" column, and "Component (E)" column of Table 1, respectively.
[0090] [Table 1]
[0091] The details of the alkyl phosphate salt (A), paraffin (B), polyoxyalkylene polyol fatty acid ester (C), nonionic surfactant (D), and other components (E) described in Table 1 are as follows.
[0092] (Alkyl phosphate salt (A)) The raw material alcohols and their carbon atom numbers used for the alkyl phosphate ester salts (A-1) to (A-5) and (a-1) to (a-4), and the types of salts constituting the alkyl phosphate ester salts are shown in the "Raw Material Alcohol" column, "Carbon Atom Number" column, and "Salt" column of Table 2 described below, respectively.
[0093] [Table 2] Ingredient(A) Raw material alcohol Number of carbon atoms Salt A-1 Ethanol 2 Potassium A-2 Propanol 3 Potassium A-3 Butanol 4 Potassium A-4 Propanol 3 Diethanolamine A-5 Butanol 4 Diethanolamine a-1 Hexanol 6 Potassium a-2 Octanol 8 Potassium a-3 Octadecanol 18 Potassium a-4 Octadecanol 18 sodium
[0094] (Paraffin (B)) B-1: Paraffin wax with a melting point of 55°C B-2: Paraffin wax with a melting point of 45°C B-3: Paraffin wax with a melting point of 65°C (Polyoxyalkylene polyol fatty acid ester (C)) C-1: Polyoxyethylene (10) sorbitan monooleate C-2: Polyoxyethylene (20) sorbitan monooctadecyl ester C-3: Polyoxyethylene (10) glycerol monooleyl ester C-4: Polyoxyethylene (20) glyceryl monooctadecyl ester C-5: Polyoxyethylene (10) 1,6-hexanediol dilauryl ester C-6: Polyoxyethylene (10) trimethylolpropane trilauryl ester (Nonionic surfactant (D)) D-1: Polyoxyethylene (18) oleyl ether D-2: Polyoxyethylene (10) lauryl ether D-3: Polyoxyethylene (10) lauryl amino ether D-4: Polyoxyethylene (7) oleyl ester D-5: Polyoxyethylene (7) stearyl ether D-6: Polyoxyethylene (5) oleyl ether (Other ingredients (E)) E-1: Diglycerol E-2: Glycerin E-3: Sorbitan monostearate E-4: Dimethyl polysiloxane E-5: Stearyl Octadecanol E-6: Potassium oleate E-7: Octadecanol Palmitate E-8: Ethylene oxide (1) butyl ether potassium phosphate (a mixture of 63% monoester, 12% diester, 8% diphosphate, and 17% inorganic phosphoric acid, acid value 20 KOHmg / g) Test Category 2 (Manufacture of synthetic fibers and nonwovens) The composition containing the treatment agent prepared in Test Category 1 was used to produce synthetic fibers and nonwoven fabrics.
[0095] The synthetic fiber used was a polyolefin-based synthetic fiber, which was composed of a composite fiber having a polyethylene sheath and a polypropylene core, and was a staple fiber having a fineness of 2.2 dtex and a length of 38 mm.
[0096] The composition containing the treatment agent of each example prepared in Test Category 1 was further diluted with water to obtain a 0.4% dilution. 100 g of the dilution was applied to 100 g of short fibers by spraying and dried in a dryer at 80°C for 1 hour. The short fibers were attached to the short fibers in such a manner that the solid content was 0.4% (without solvent).
[0097] In addition, 20 g of the dried synthetic fibers were formed into a carded web using a known small drum carding machine at a temperature of 25°C and a humidity of 40%. The carded web was subjected to a hot air treatment at 140°C for 10 seconds to bond the fibers to produce a carded web weighing 25 g / m 2 of non-woven fabric.
[0098] The compositions containing the treatment agent of each example obtained above were used to evaluate stability, the short fiber samples obtained were used to evaluate antistatic properties, and the nonwoven fabric samples obtained were used to evaluate water repellency.
[0099] Test category 3 (Evaluation of water repellency) The evaluation of water repellency is carried out according to the hydrostatic pressure method of method A (low water pressure method) described in 7.1.1 of JIS L 1092. Among them, the description of the hydrostatic pressure method in JIS L 1092 corresponds to the international standard ISO811. The water pressure measuring instrument is made by TEXTEST, Switzerland (FX3000-III). The test environment is a temperature of 20±2°C and a humidity of 65±2%RH. Take 5 pieces of non-woven fabrics made in test category 2 (about 150mm×about 150mm) and install them on the water pressure measuring instrument so that the surface side of the non-woven fabric is in contact with water. The water level is raised at a speed of 10cm / min, and the displayed value (cmw.c.) is read when the third drop of water appears on the inside of the non-woven fabric. The test is performed 5 times, and the average value of the 5 times is calculated. The higher the water pressure resistance, the better the water repellency. Among them, very small water droplets that do not grow larger after appearing on the inner side of the nonwoven fabric, or water droplets formed by passing through the same position are not included in the calculation. The test results are shown in the "Water Repellency" column of Table 1.
[0100] ·Evaluation criteria for water repellency ◎(Good): Water pressure resistance is 3.0cmw.c. or above ○ (Acceptable): Water pressure resistance is 1.0 cmw.c. or more but less than 3.0 cmw.c. × (bad): Water pressure resistance less than 1.0 cmw.c. Test Category 4 (Evaluation of Antistatic Properties) 20 g of the short fibers produced in Test Category 2 were formed into a carded web using a small drum carding machine under low humidity conditions of 20°C and 30% relative humidity. The voltage of static electricity generated by the carded web at the exit of the carding machine under low humidity was measured and evaluated using the evaluation criteria described below. The test results are shown in the "Antistatic Properties" column of Table 1.
[0101] Evaluation criteria for antistatic properties ◎(Good): The voltage generating static electricity is less than 500V ○ (Acceptable): The voltage generating static electricity is 500V or more but less than 1kV × (bad): The voltage of static electricity generated is 1 kV or more Test Category 5 (Evaluation of Stability) The solution stability of the dilution of the treatment agent was evaluated as a surrogate evaluation for scum generation. The composition containing the treatment agent (40% treatment agent) of each example prepared in Test Category 1 was further diluted with water to prepare a 1% dilution. The 1% dilution was placed in a sealed container and allowed to stand for 24 hours at 5°C, 20°C, and 50°C. After standing for 24 hours, the state of the solution at each temperature was visually observed and evaluated using the following evaluation criteria. The test results are shown in the "Stability" column of Table 1.
[0102] Stability evaluation criteria ◎ (good): No precipitate or separation was observed in any of the dilutions. ○ (Acceptable): A very small amount of precipitate or separation was observed in any of the dilutions. × (bad): precipitate or separation was observed in any of the dilutions Test category 6 (preparation of a composition containing the first treatment agent) (Composition (1-1) containing the first treatment agent) As shown in Table 3, 86 parts (%) of paraffin wax (B-1) having a melting point of 55°C, 7 parts (%) of polyoxyethylene (10) sorbitan monooleyl ester (C-1) of polyoxyalkylene polyol fatty acid ester (C), and 7 parts (%) of polyoxyethylene (18) oleyl ether (D-1) of nonionic surfactant (D) were weighed and added to a container. These were stirred and mixed uniformly at a temperature of about 80°C. Furthermore, 100 parts of 20°C water as a solvent (S) was added to the container while being stirred and mixed uniformly, making a total of 200 parts. Then, emulsification was performed to prepare a composition (1-1) containing 50% of the first treatment agent.
[0103] (Compositions (1-2) to (1-25) containing the first treatment agent) Compositions (1-2) to (1-25) containing a first treatment agent are prepared in the same manner as the composition (1-1) containing a first treatment agent, and contain paraffin (B), polyoxyalkylene polyol fatty acid ester (C), nonionic surfactant (D), other components (E), and a solvent (S) in the proportions shown in Table 3.
[0104] The type and content of paraffin (B), the type and content of polyoxyalkylene polyol fatty acid ester (C), the type and content of nonionic surfactant (D), the type and content of other components (E), and the type and content of solvent (S) are shown in the "Component (B)" column, "Component (C)" column, "Component (D)" column, "Component (E)" column, and "Solvent (S)" column of Table 3, respectively.
[0105] [Table 3]
[0106] Test Category 7 (Preparation of a composition containing a second treatment agent) (Composition (2-1) containing the second treatment agent) As shown in Table 4, 100 parts of potassium salt of ethyl phosphate (A-1) of alkyl phosphate (A) and 100 parts of 20°C water (S) of solvent (S) were added and stirred uniformly, and the total amount was 200 parts. Then, emulsification was performed to prepare a composition (2-1) containing 50% of the second treatment agent.
[0107] (Compositions (2-2) to (2-5) containing the second treatment agent) Compositions (2-2) to (2-5) containing the second treatment agent were prepared, which contained the alkyl phosphate ester salt (A) and the solvent (S) in the ratio shown in Table 4. The type and content of the alkyl phosphate ester salt (A), and the type and content of the solvent (S) are shown in the "Component (A)" column and the "Solvent (S)" column of Table 4, respectively.
[0108] [Table 4]
[0109] Test Category 8 (Evaluation of Stability of Preparations) After the preparation of the above-mentioned compositions containing the first treatment agent and the second treatment agent, they were transferred to a sealable container and allowed to stand at 20°C for 24 hours, and then their appearances were visually evaluated using the following criteria. The results are shown in the "Preparation Stability" column of Tables 3 and 4.
[0110] · Evaluation criteria for formulation stability (composition containing the first treatment agent and composition containing the second treatment agent) ◎(Good): No separation or precipitation is observed and the surface is uniform. ○ (Acceptable): A few particles are seen but there is no problem in using it × (bad): Severe precipitation or product separation and problems in use Test Category 9 (Preparation of a dilution solution of a treatment agent consisting of a composition containing a first treatment agent and a composition containing a second treatment agent) (Examples 26 to 50) In a 1000 mL beaker prepared with 80°C ion exchange water, add a composition containing the first treatment agent and a composition containing the second treatment agent in the ratios described in Examples 26 to 50 of Table 5. At this time, the total amount of the composition containing the first treatment agent and the composition containing the second treatment agent is 100 g, that is, the total amount of the first treatment agent and the second treatment agent added is 50 g. Finally, a 5% dilution of the treatment agent is prepared. Among them, the amount of 80°C ion exchange water prepared in advance can be appropriately adjusted depending on the concentration or usage of the composition containing the first treatment agent and the composition containing the second treatment agent, so that the content ratio of the treatment agent for short fibers becomes 5%.
[0111] Using the obtained diluted solution of the treatment agent of each example, water repellency, antistatic property and stability were evaluated in the same manner as in Example 1. The results are shown in the "Water Repellency" column, the "Antistatic Property" column and the "Stability" column of Table 5, respectively.
[0112] [Table 5]
[0113] It is clear from the evaluation results of each embodiment with respect to the comparative example in Table 1 that the treatment agent of the present invention can improve stability. In addition, the water repellency and antistatic properties imparted by the treatment agent to the synthetic fiber can be improved. In addition, the first treatment agent and the second treatment agent of the present invention can improve the formulation stability.
[0114] The present disclosure also includes the following aspects. (Appendix 1) A processing agent for short fibers, characterized in that: It contains the component (A) described below, the component (B) described below, and the component (C) described below.
[0115] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester.
[0116] (Appendix 2) The short fiber treating agent as described in Appendix 1, wherein The nonvolatile content of the short fiber processing agent contains 5% to 50% by mass of the component (A), 40% to 70% by mass of the component (B), and 2% to 10% by mass of the component (C).
[0117] (Appendix 3) The short fiber treating agent as described in Appendix 1 or 2, wherein Furthermore, it contains the component (D) mentioned later. Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C).
[0118] (Appendix 4) The short fiber treating agent as described in Appendix 3, wherein: The nonvolatile content of the short fiber processing agent contains the component (D) in an amount of 2% by mass or more and 10% by mass or less.
[0119] (Appendix 5) The short fiber processing agent as described in Appendix 3 or 4, wherein The non-volatile component of the above-mentioned short fiber processing agent contains the above-mentioned component (A) at least 20 mass % and less than 40 mass %, the above-mentioned component (B) at least 45 mass % and less than 65 mass %, the above-mentioned component (C) at least 4 mass % and less than 8 mass %, and the above-mentioned component (D) at least 4 mass % and less than 8 mass %.
[0120] (Appendix 6) The short fiber treating agent as described in Appendix 1 or 2, wherein The present invention comprises a first treatment agent for short fibers and a second treatment agent for short fibers in combination, wherein the first treatment agent for short fibers contains the component (B), the component (C), and optionally contains the component (D), and the second treatment agent for short fibers contains the component (A).
[0121] Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C). (Appendix 7) A composition containing a short fiber treating agent, characterized in that: Contains the short fiber processing agent and a solvent as described in any one of Appendices 1 to 6.
[0122] (Appendix 8) A first treatment agent for short fibers, which, when used, is used together with a second treatment agent for short fibers containing component (A) described later, and when not used, is constituted in a different agent form from the second treatment agent for short fibers, characterized in that: It contains the component (B) and the component (C) described below, and optionally contains the component (D) described below.
[0123] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester.
[0124] Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C). (Appendix 9) A second treatment agent for staple fibers, which, when used, is used together with a first treatment agent for staple fibers containing the component (B) and the component (C) described below, and optionally containing the component (D) described below, and when not used, is a different agent from the first treatment agent for staple fibers, It is characterized in that Contains the component (A) described below.
[0125] Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms. Ingredient (B): Paraffin. Ingredient (C): polyoxyalkylene polyol fatty acid ester.
[0126] Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C). (Appendix 10) A composition containing a first treatment agent for short fibers, characterized in that: Contains the first treatment agent for short fibers described in Appendix 8 and a solvent.
[0127] (Appendix 11) A composition containing a second treatment agent for short fibers, characterized in that: Contains the second treatment agent for short fibers described in Appendix 9 and a solvent.
[0128] (Appendix 12) A synthetic fiber, characterized in that The short fiber processing agent described in any one of Appendixes 1 to 6 is attached.
[0129] (Appendix 13) A method for manufacturing a nonwoven fabric, characterized in that: Go through steps 1 to 3 described below. Step 1: Make the short fiber treatment agent described in any one of Appendices 1 to 6 adhere to the synthetic fiber.
[0130] Step 2: The synthetic fibers to which the short fiber treating agent is attached in the above step 1 are passed through a carding machine to obtain a carded web. Step 3: The carded web obtained in the above step 2 is subjected to a heat fusion treatment to obtain a nonwoven fabric.
[0131] (Appendix 14) The method for manufacturing a nonwoven fabric as described in Appendix 13, wherein: The synthetic fibers are polyolefin-based synthetic fibers.
Claims
1. A short fiber treatment agent, characterized in that: Contains the component (A) described below, the component (B) described below, and the component (C) described below, The nonvolatile component of the short fiber treatment agent contains 5% by mass or more and 50% by mass of the component (A), 30% by mass or more and 75% by mass of the component (B), and 2% by mass or more and 15% by mass of the component (C), Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms, Ingredient (B): Paraffin, Ingredient (C): polyoxyalkylene polyol fatty acid ester.
2. The short fiber processing agent according to claim 1, wherein The short fiber processing agent contains 40% by mass to 70% by mass of the component (B) and 2% by mass to 10% by mass of the component (C) in the nonvolatile content.
3. The short fiber processing agent according to claim 1 or 2, wherein: Furthermore, it contains the component (D) described later, Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C).
4. The short fiber processing agent according to claim 3, wherein The nonvolatile content of the short fiber processing agent contains the component (D) in an amount of 2% by mass or more and 10% by mass or less.
5. The short fiber processing agent according to claim 3 or 4, wherein The non-volatile component of the above-mentioned short fiber processing agent contains the above-mentioned component (A) at least 20 mass % and less than 40 mass %, the above-mentioned component (B) at least 45 mass % and less than 65 mass %, the above-mentioned component (C) at least 4 mass % and less than 8 mass %, and the above-mentioned component (D) at least 4 mass % and less than 8 mass %.
6. A staple fiber treatment agent kit, comprising a first staple fiber treatment agent and a second staple fiber treatment agent in combination, wherein the first staple fiber treatment agent contains the component (B) and the component (C) described below, and optionally contains the component (D) described below, and the second staple fiber treatment agent contains the component (A) described below, When the first treatment agent for short fibers and the second treatment agent for short fibers are mixed, the nonvolatile component of the obtained treatment agent for short fibers contains 5% by mass or more and 50% by mass of the component (A), 30% by mass or more and 75% by mass of the component (B), and 2% by mass or more and 15% by mass of the component (C), Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms, Ingredient (B): Paraffin, Ingredient (C): polyoxyalkylene polyol fatty acid ester, Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, wherein: Exclude those meeting component (C).
7. A composition containing a short fiber treatment agent, characterized in that: The method comprises the short fiber treating agent according to any one of claims 1 to 5 and a solvent.
8. A composition containing a short fiber treatment agent, characterized in that , Contains the first short fiber treating agent, the second short fiber treating agent, and a solvent in the short fiber treating agent kit according to claim 6.
9. A first treatment agent for short fibers, which, when used, is used together with a second treatment agent for short fibers containing component (A) described later, and when not used, is constituted in a different agent form from the second treatment agent for short fibers, characterized in that: The invention contains the component (B) and the component (C) described later, and optionally contains the component (D) described later, and when the first treatment agent for short fibers and the second treatment agent for short fibers are mixed, the non-volatile component of the treatment agent for short fibers obtained contains 5% by mass or more and 50% by mass of the component (A), 30% by mass or more and 75% by mass of the component (B), and 2% by mass or more and 15% by mass of the component (C), Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms, Ingredient (B): Paraffin, Ingredient (C): polyoxyalkylene polyol fatty acid ester, Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C).
10. A second treatment agent for staple fibers, which when used is used together with a first treatment agent for staple fibers containing the component (B) and the component (C) described later, and optionally containing the component (D) described later, and when not used is constituted in a different agent form from the first treatment agent for staple fibers, characterized in that: The invention contains the component (A) described later, and when the first treatment agent for staple fibers and the second treatment agent for staple fibers are mixed, the non-volatile matter of the obtained treatment agent for staple fibers contains 5% by mass or more and 50% by mass of the component (A), 30% by mass or more and 75% by mass of the component (B), and 2% by mass or more and 15% by mass of the component (C), Component (A): an alkyl phosphate having an alkyl group having 1 to 5 carbon atoms, Ingredient (B): Paraffin, Ingredient (C): polyoxyalkylene polyol fatty acid ester, Component (D): a nonionic surfactant having a (poly)oxyalkylene structure in the molecule, excluding those corresponding to component (C).
11. A composition containing a first treatment agent for short fibers, characterized in that , Contains the first treatment agent for short fibers according to claim 9 and a solvent.
12. A composition containing a second treatment agent for short fibers, characterized in that , Contains the second treatment agent for short fibers according to claim 10 and a solvent.
13. A synthetic fiber, characterized in that: The short fiber processing agent according to any one of claims 1 to 5 is attached.
14. A synthetic fiber, characterized in that: A short fiber treating agent is attached, wherein the short fiber treating agent is a mixture of the first short fiber treating agent and the second short fiber treating agent in the short fiber treating agent set according to claim 6.
15. A method for producing a nonwoven fabric, characterized in that: Through the following steps 1 to 3, Step 1: attaching the short fiber treatment agent according to any one of claims 1 to 5 to synthetic fibers, Step 2: passing the synthetic fiber to which the short fiber treatment agent is attached in the above step 1 through a carding machine to obtain a carded web, Step 3: The carded web obtained in the above step 2 is subjected to a heat fusion treatment to obtain a nonwoven fabric.
16. A method for producing a nonwoven fabric, characterized in that: Through the following steps 1 to 3, Step 1: attaching a short fiber treatment agent to the synthetic fiber, wherein the short fiber treatment agent is a mixture of the first short fiber treatment agent and the second short fiber treatment agent in the short fiber treatment agent set according to claim 6, Step 2: passing the synthetic fiber to which the short fiber treatment agent is attached in the above step 1 through a carding machine to obtain a carded web, Step 3: The carded web obtained in the above step 2 is subjected to a heat fusion treatment to obtain a nonwoven fabric.
17. The method for producing a nonwoven fabric according to claim 15 or 16, wherein: The synthetic fibers are polyolefin-based synthetic fibers.
Citation Information
Patent Citations
Fiber treating agent for staple fibers, and use for said agent
WO2017199702A1
Agent for treating short-staple fibers and use for said agent
CN105793486A
Processing agents and methods for synthetic fibers
CN1704522A
Fiber-treating agent, short polyester fiber made with the same, and nonwoven fabric
CN1934308A
A method of processing synthetic fibers, synthetic fibers, a method of spinning synthetic fibers and spun yarn