Lithium ion battery fire extinguishing agent and preparation method thereof

Through the mixing of MIL-96-Al/GO composite material and perfluorohexanone, the problem of poor cooling performance and corrosion of perfluorohexanone fire extinguishing agent in lithium-ion battery fires is solved, and efficient extinguishing of lithium-ion battery fires is achieved. and improve corrosion resistance, providing an efficient fire extinguishing agent.

CN118987553AActive Publication Date: 2024-11-22STATE GRID ANHUI ELECTRIC POWER CO LTD ELECTRIC POWER SCI RES INST +1

Patent Information

Application Number
CN202411084983.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing perfluorohexanone fire extinguishing agent has poor cooling performance and is prone to corrosion in lithium-ion battery fires, which cannot effectively solve the problem of rekindling of lithium-ion battery fires.

Method used

MIL-96-Al/GO composite material and perfluorohexanone are used to prepare MIL-96-Al/GO through hydrothermal reaction, and stir with perfluorohexanone and sonicate to form a kind of lithium Ion battery fire extinguishing agent improves its cooling performance and corrosion resistance.

Benefits of technology

It significantly improves the heat of vaporization and corrosion resistance of perfluorohexanone, enhances the extinguishing ability and continuous heat absorption capacity of lithium-ion batteries, avoids the problem of rekindling of lithium-ion batteries, and provides a high-efficiency and corrosion-free fire extinguishing agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987553A_ABST
    Figure CN118987553A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium ion battery fire extinguishing agent and a preparation method thereof. The fire extinguishing agent comprises the following raw materials: MIL-96-Al / GO and perfluorohexanone; the preparation process of the MIL-96-Al / GO comprises the following steps: uniformly mixing and dispersing graphene oxide, water and MIL-96-Al, then carrying out hydrothermal reaction, cooling, collecting a solid, and drying to obtain the MIL-96-Al / GO. According to the invention, MIL-96-Al and graphene oxide are compounded to obtain the composite material MIL-96-Al / GO, and the composite material MIL-96-Al / GO can be uniformly dispersed in the perfluorohexanone and directly adsorb fluorine ions in the long-term storage process of the perfluorohexanone, so that the problem of corrosivity of the perfluorohexanone is solved. In addition, the composite material can greatly improve the vaporization heat of the perfluorohexanone, so that the perfluorohexanone has excellent continuous heat absorption capacity, the problem that the lithium ion battery is easy to reburn can be well solved, and the prepared fire extinguishing agent is an efficient fire extinguishing agent which is insulated, strong in heat absorption and free of corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of materials, and in particular to a lithium ion battery fire extinguishing agent and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantages of good cycle performance, no memory effect, and high specific energy. They are widely used in electric vehicles, electrochemical energy storage, and other electronic products. my country is currently the largest producer and user of lithium-ion batteries, and is vigorously developing lithium-ion battery technology. The large-scale application of lithium-ion batteries is an important support for achieving the dual-carbon strategic goals. However, lithium-ion batteries are an energetic substance with a dangerous nature. When squeezed by the outside world or abused by electricity or heat, they are prone to thermal runaway and then fire or even explosion. Especially indoors or in energy storage system containers, the fire load is large, the risk is high, and it is difficult to extinguish.

[0003] Lithium-ion battery fires are different from conventional fires. They have many fire characteristics, such as fast ignition speed, long duration, and extremely high combustion temperature. They can even ignite the inside of the battery module and other combustible materials, causing a larger fire, and are prone to reignition. Existing fire extinguishing agents such as heptafluoropropane and carbon dioxide cannot solve the problem of lithium-ion battery fires that are prone to reignition. Water is prone to secondary disasters and cannot be used as a lithium-ion battery fire extinguishing agent. Perfluorohexanone, which is currently widely used, has a certain effect on lithium-ion battery fires, but on the one hand, perfluorohexanone is prone to produce fluoride ions during long-term storage and release of fire extinguishing, and then combines with moisture in the environment to produce hydrofluoric acid, causing corrosiveness. On the other hand, perfluorohexanone has a low heat of vaporization and poor cooling performance, and lithium-ion batteries are also prone to reignition.

[0004] The method to solve the corrosiveness and poor cooling performance of perfluorohexanone is to introduce other additives. For example, in the Chinese patent application document with publication number CN113209537A, heptafluorocyclopentane is introduced into perfluorohexanone as a method to improve the cooling performance. 2H-MIL-125 (Ti) is used as an adsorption additive for water and HF, thereby improving the corrosion resistance and cooling performance of perfluorohexanone. In the Chinese patent application document with publication number CN113350730A, perfluorohexanone is also used as a fire extinguishing material, and other fluorine-containing organic substances with high vaporization heat are introduced as cooling materials and aluminum oxide is used as an anti-corrosion material to improve the cooling ability and corrosion resistance of perfluorohexanone as a lithium-ion battery fire extinguishing agent. The above patent documents all solve the corrosive problem of perfluorohexanone by introducing different additives, and at the same time introduce other materials with high vaporization heat to improve the cooling performance of perfluorohexanone, and all involve the mixing of three or more substances. The multiple substances include liquids and solids, and the fluidity and permeability of the mixed fire extinguishing agent may be affected, and the interface bonding of liquid and solid materials is a challenge. During long-term storage, there are solid precipitation and liquid stratification, which affects the performance of the fire extinguishing agent. Summary of the invention

[0005] The technical problem to be solved by the present invention is how to improve the corrosion resistance and cooling performance of perfluorohexanone fire extinguishing agent.

[0006] The present invention solves the above technical problems through the following technical means:

[0007] A lithium-ion battery fire extinguishing agent, the raw materials of which include MIL-96-Al / GO and perfluorohexanone; the preparation process of the MIL-96-Al / GO includes the following steps: mixing and dispersing graphene oxide, water and MIL-96-Al evenly, then performing a hydrothermal reaction, collecting solids after cooling, and drying to obtain the MIL-96-Al / GO.

[0008] Preferably, the usage ratio of the MIL-96-Al / GO to perfluorohexanone is 5-30 mg:100 ml.

[0009] Preferably, the MIL-96-Al is prepared by a hydrothermal reaction using aluminum nitrate as a metal salt, trimesic acid as a ligand, and water as a solvent.

[0010] Preferably, the usage ratio of graphene oxide to water is 5-20 mg:50 ml.

[0011] Preferably, the mass ratio of the graphene oxide to MIL-96-Al is 5 to 20:100.

[0012] Preferably, the process of uniformly mixing and dispersing graphene oxide, water and MIL-96-Al includes mixing graphene oxide and water, ultrasonically dispersing for 1 to 5 hours, adding MIL-96-Al, and ultrasonically dispersing for 1 to 2 hours.

[0013] Preferably, in the preparation process of MIL-96-Al / GO, the temperature of the hydrothermal reaction is 100-150° C., and the time is 6-12 hours.

[0014] The present invention also provides a method for preparing the lithium-ion battery fire extinguishing agent, comprising the following steps: mixing MIL-96-Al / GO and perfluorohexanone, stirring, and then ultrasonically treating to obtain the lithium-ion battery fire extinguishing agent.

[0015] Preferably, the stirring is stirring at room temperature; and the stirring time is greater than or equal to 6 hours.

[0016] Preferably, the ultrasonic treatment time is 1 to 3 hours and the temperature does not exceed 30°C.

[0017] The advantages of the present invention are:

[0018] The MIL-96-Al in the present invention is a porous organic framework material with good chemical stability and thermal stability. By compounding with graphene oxide GO, a composite material MIL-96-Al / GO is obtained, which can be uniformly dispersed in perfluorohexanone, can solve the agglomeration of particles in perfluorohexanone, and directly adsorb fluoride ions during the long-term storage of perfluorohexanone, thereby solving the problem of the corrosiveness of perfluorohexanone; in addition, the addition of MIL-96-Al / GO solid matter can increase the interaction between perfluorohexanone solvent molecules and MIL-96-Al / GO, thereby enhancing the cohesive force between perfluorohexanone molecules, greatly improving the vaporization heat of perfluorohexanone, and at the same time, with the addition of solid particles, the vapor pressure of the perfluorohexanone solvent will decrease, which means that a greater phase change resistance needs to be overcome during the vaporization process. Therefore, more energy is required to vaporize the solvent, which also leads to an increase in vaporization heat, so that perfluorohexanone has excellent continuous heat absorption capacity, which can well solve the problem of easy re-ignition of lithium-ion batteries. The lithium-ion battery fire extinguishing agent prepared by the present invention is an efficient fire extinguishing agent with strong insulation, heat absorption and no corrosion, and can be used as a fire extinguishing agent in live scenes. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 XRD patterns of MIL-96-Al, GO and MIL-96-Al / GO in Example 1 of the present invention;

[0020] Figure 2 is a SEM image of MIL-96-Al / GO in Example 1 of the present invention;

[0021] Figure 3 is the adsorption curve of fluoride ions by MIL-96-Al / GO in Example 1 of the present invention;

[0022] Figure 4Schematic diagram of the battery box and battery arrangement used in the performance test process of the present invention. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0025] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0026] Example 1

[0027] A method for preparing a lithium-ion battery fire extinguishing agent comprises the following steps:

[0028] (1) Preparation of MIL-96-Al

[0029] Weigh 3g of aluminum nitrate nonahydrate and 3g of trimesic acid and add them to 50ml of pure water. Keep stirring in a glass beaker until the solid is completely dissolved in the water. Then transfer to a 100ml polytetrafluoroethylene reactor, put it in a drying oven, heat it to 250℃ and react for 36h. After cooling to room temperature naturally, collect the obtained powder product by centrifugation. At the same time, wash it three times with pure water by centrifugation to remove the residual substances in the product, and then transfer it to an 80℃ drying oven for drying for 15h to obtain the required MIL-96-Al.

[0030] (2) Preparation of MIL-96-Al / GO

[0031] Weigh 20 mg of graphene oxide GO and dissolve it in 50 ml of pure water, place it in a CNC ultrasonic cleaner and ultrasonically vibrate for 5 hours to fully disperse GO in water. Take 100 mg of the synthesized MIL-96-Al and add it, continue ultrasonic oscillation for 2 hours, and after the MIL-96-Al powder is fully mixed with GO, transfer it to a 100 ml polytetrafluoroethylene reactor, put it in a drying oven, heat it to 150 ° C for 12 hours, cool it naturally to room temperature, collect the powder product by centrifugation, and transfer it to a drying oven at 80 ° C for 12 hours to obtain the required MIL-96-Al / GO.

[0032] (3) Preparation of fire extinguishing agent

[0033] Weigh 24 mg of MIL-96-Al / GO powder and add it to 100 ml of perfluorohexanone in a round-bottom flask. Seal the round-bottom flask with a stopper and stir at room temperature for 10 h to evenly disperse the MIL-96-Al / GO powder in the perfluorohexanone solution. Then transfer it to an ultrasonic cleaner and ultrasonicate it for 3 h. During the ultrasonication process, add ice cubes to the cleaner from time to time to control the water temperature in the cleaner not to exceed 30 °C.

[0034] Figure 1 The XRD pattern shown is that of MIL-96-Al / GO prepared in Example 1. Compared with the XRD patterns of MIL-96-Al and GO, Figure 1 It can be seen that the three characteristic peaks of GO are in the range of 2θ=15~30. After combining with GO, MIL-96-Al / GO (as shown in the figure MIL-96-Al@GO) simultaneously shows the characteristic peaks of MIL-96-Al and GO, indicating that MIL-96-Al and GO are successfully combined together.

[0035] pass Figure 2 The overall morphology of MIL-96-Al / GO was observed by SEM, and the nanosheet structure of GO used was clearly seen. The MIL-96-Al was uniformly dispersed on GO and well combined with GO.

[0036] Example 2

[0037] A method for preparing a lithium-ion battery fire extinguishing agent comprises the following steps:

[0038] (1) Preparation of MIL-96-Al

[0039] Weigh 2g of aluminum nitrate nonahydrate and 2g of trimesic acid and add them to 50ml of pure water. Keep stirring in a glass beaker until the solid is completely dissolved in the water. Then transfer to a 100ml polytetrafluoroethylene reactor, put it in a drying oven, heat it to 200℃ and react for 24h. After cooling naturally to room temperature, collect the obtained powder product by centrifugation. At the same time, wash it three times with pure water by centrifugation. After removing the residual substances in the product, transfer it to a 120℃ drying oven for drying for 12h to obtain the required MIL-96-Al.

[0040] (2) Preparation of MIL-96-Al / GO

[0041] Weigh 5 mg of graphene oxide GO and dissolve it in 50 ml of pure water, place it in a CNC ultrasonic cleaner and ultrasonically vibrate for 3 hours to fully disperse GO in water. Take 100 mg of the synthesized MIL-96-Al and add it, continue ultrasonic oscillation for 1 hour, and after the MIL-96-Al powder is fully mixed with GO, transfer it to a 100 ml polytetrafluoroethylene reactor, put it in a drying oven, heat it to 120 ° C to react for 8 hours, cool it naturally to room temperature, collect the powder product by centrifugation, and transfer it to a 120 ° C drying oven for drying for 12 hours to obtain the required MIL-96-Al / GO.

[0042] (3) Preparation of fire extinguishing agent

[0043] Weigh 16 mg of MIL-96-Al / GO powder and add it to 100 ml of perfluorohexanone in a round-bottom flask. Seal the round-bottom flask with a stopper and stir at room temperature for 6 hours to evenly disperse the MIL-96-Al / GO powder in the perfluorohexanone solution. Then transfer it to an ultrasonic cleaner and ultrasonicate it for 2 hours. During the ultrasonication process, add ice cubes to the cleaner from time to time to control the water temperature in the cleaner not to exceed 30°C.

[0044] Example 3

[0045] A method for preparing a lithium-ion battery fire extinguishing agent comprises the following steps:

[0046] (1) Preparation of MIL-96-Al

[0047] Weigh 2.5g aluminum nitrate nonahydrate and 2.5g trimesic acid and add them to 50ml pure water. Keep stirring in a glass beaker until the solid is completely dissolved in the water. Then transfer to a 100ml polytetrafluoroethylene reactor, put it in a drying oven, heat it to 180℃ for 12h, cool it naturally to room temperature and collect the powder product by centrifugation. At the same time, wash it three times with pure water by centrifugation to remove the residual substances in the product, and then transfer it to a 100℃ drying oven for drying for 12h to obtain the required MIL-96-Al.

[0048] (2) Preparation of MIL-96-Al / GO

[0049] Weigh 10 mg of graphene oxide GO and dissolve it in 50 ml of pure water, place it in a CNC ultrasonic cleaner for ultrasonic vibration for 1 hour, so that GO is fully dispersed in water. Take 100 mg of MIL-96-Al synthesized above and add it, continue ultrasonic vibration for 1.5 hours, after the MIL-96-Al powder is fully mixed with GO, transfer it to a 100 ml polytetrafluoroethylene reactor, put it in a drying oven, heat it to 100 ° C and react for 6 hours, cool it naturally to room temperature, collect the powder product by centrifugation, transfer it to a drying oven at 80 ° C and dry it for 12 hours, and obtain the required MIL-96-Al / GO.

[0050] (3) Preparation of fire extinguishing agent

[0051] Weigh 8 mg of MIL-96-Al / GO powder and add it to 100 ml of perfluorohexanone in a round-bottom flask. Seal the round-bottom flask with a stopper and stir at room temperature for 8 h to evenly disperse the MIL-96-Al / GO powder in the perfluorohexanone solution. Then transfer it to an ultrasonic cleaner and ultrasonicate it for 1 h. During the ultrasonication process, add ice cubes to the cleaner from time to time to control the water temperature in the cleaner not to exceed 30°C.

[0052] Comparative Example 1

[0053] The difference from Example 1 is that only step (1) and step (3) of Example 1 are included, and in step (3), the MIL-96-Al prepared in step (1) is used to replace the MIL-96-Al / GO powder to prepare the fire extinguishing agent.

[0054] Comparative Example 2

[0055] Preparation of fire extinguishing agent

[0056] Weigh 24 mg of GO powder and add it to 100 ml of perfluorohexanone in a round-bottom flask. Seal the round-bottom flask with a stopper and stir at room temperature for 10 h to evenly disperse the GO powder in the perfluorohexanone solution. Then transfer it to an ultrasonic cleaner and ultrasonicate for 3 h. During the ultrasonication process, add ice cubes to the cleaner from time to time to control the water temperature in the cleaner not to exceed 30 °C.

[0057] Comparative Example 3

[0058] Preparation of fire extinguishing agent

[0059] The difference from Example 1 is that only step (1) and step (3) of Example 1 are included, and in step (3), a mixture of MIL-96-Al and graphene oxide prepared in step (1) is used to replace the MIL-96-Al / GO powder to prepare the fire extinguishing agent, wherein the mass ratio of MIL-96-Al to graphene oxide is 5:1.

[0060] The fire extinguishing agents of Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the specific test methods are as follows:

[0061] A handheld fire extinguisher was used to manually start the spraying to verify the suppression of thermal runaway of lithium batteries by the fire extinguishing agent and perfluorohexanone of the present invention. The amount of fire extinguishing agent used was 1500 ml.

[0062] 1) Test cell type: square aluminum shell lithium iron phosphate battery, specification 3.2V 280Ah;

[0063] 2) Thermal runaway triggering method: Heating method triggers thermal runaway;

[0064] 3) Start mode: manual start;

[0065] 4) Test box: stainless steel shell, the size is 840mm long, 335mm wide, and 150mm high (temperature and voltage detectors are arranged at the battery cell to record thermal runaway test data), as shown in the schematic diagram Figure 4 As shown;

[0066] The comparison of the fire extinguishing process of perfluorohexanone and pure perfluorohexanone fire extinguishing agents under different MIL-96-Al / GO addition amounts in Example 1-3 is shown in Table 1 below;

[0067] Table 1

[0068]

[0069] Table 2 Comparison of fire extinguishing process of fire extinguishing agent in comparative examples 1-3

[0070] Pure perfluorohexanone Comparative Example 1 Comparative Example 2 Comparative Example 3 Flame disappearance time / s 12s 6s 7s 9s Whether relapse occurs yes yes yes yes The time it takes for the flame to reignite after it is extinguished 35s 51s 42s 46s

[0071] Table 3 Comparison of cooling process of perfluorohexanone fire extinguishing agent under different MIL-96-Al / GO addition amounts in Example 1-3

[0072]

[0073] Table 4 Comparison of the cooling process of the fire extinguishing agent in Comparative Examples 1-3

[0074]

[0075]

[0076] From the comparison results in Tables 1 to 4, we can see that with the increase in the amount of MIL-96-Al / GO added, the speed of extinguishing open flames, the ability to continuously cool down, and the effect of inhibiting re-ignition of modified perfluorohexanone on lithium-ion battery fires are greatly improved. This fully demonstrates the role of MIL-96-Al / GO in improving the performance of perfluorohexanone.

[0077] At the same time, in order to understand the corrosion effect of the fire extinguishing agent, Q335 steel plates were selected as the observation objects. 100g of Q335 steel plates were immersed in perfluorohexanone fire extinguishing agents with different MIL-96-Al / GO addition amounts for 30 days. The steel plates were taken out, dried and weighed to observe the changes in the mass of the steel plates.

[0078] Table 5 Corrosion resistance of fire extinguishing agent at different MIL-96-Al / GO addition amounts

[0079]

[0080] With the increase of MIL-96-Al / GO addition, the mass loss of the steel plate gradually decreased, which fully demonstrated the improvement effect of MIL-96-Al / GO on the corrosion resistance of perfluorohexanone.

[0081] Table 6 Physical properties of pure perfluorohexanone and the fire extinguishing agent of Example 1

[0082]

[0083] Adsorption test method for free fluoride ions: According to the experimental requirements, a 0.01 mol / L fluoride ion standard solution is prepared with sodium fluoride, 24 mg of the MIL-96-Al / GO powder prepared in Example 1 is weighed and added to 100 ml of the fluoride ion standard solution, and the solution is allowed to stand for a period of time. Within a predetermined time interval, a small amount of the suspension is taken out for centrifugal treatment to separate the supernatant, and the fluoride ion concentration in the supernatant is determined using a fluoride ion selective electrode, and the data is recorded to calculate the adsorption efficiency of the powder for fluoride ions. The results are as follows: Figure 3 As shown, from Figure 3 It can be seen that the MIL-96-Al / GO prepared by the present invention has a strong adsorption efficiency for free fluoride ions. Within 100 seconds, the adsorption efficiency for free fluoride ions is as high as 98%.

[0084] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A lithium-ion battery fire extinguishing agent, characterized in that: The raw materials include MIL-96-Al / GO and perfluorohexanone; the preparation process of MIL-96-Al / GO The method comprises the following steps: mixing and dispersing graphene oxide, water and MIL-96-Al uniformly, then performing a hydrothermal reaction, collecting solids after cooling, and drying to obtain the MIL-96-Al / GO.

2. The lithium-ion battery fire extinguishing agent according to claim 1, characterized in that: The usage ratio of the MIL-96-Al / GO to perfluorohexanone is 5-30 mg:100 ml.

3. The lithium-ion battery fire extinguishing agent according to claim 1, characterized in that: The MIL-96-Al is prepared by hydrothermal reaction with aluminum nitrate as metal salt, trimesic acid as ligand and water as solvent.

4. The lithium-ion battery fire extinguishing agent according to claim 1, characterized in that: The usage ratio of graphene oxide to water is 5-20 mg:50 ml.

5. The lithium-ion battery fire extinguishing agent according to claim 1, characterized in that: The mass ratio of the graphene oxide to MIL-96-Al is 5 to 20:

100.

6. The lithium-ion battery fire extinguishing agent according to claim 1, characterized in that: The process of uniformly mixing and dispersing graphene oxide, water and MIL-96-Al includes mixing graphene oxide and water, ultrasonically dispersing for 1 to 5 hours, adding MIL-96-Al, and ultrasonically dispersing for 1 to 2 hours.

7. The lithium ion battery fire extinguishing agent according to any one of claims 1 to 6, characterized in that: In the preparation process of MIL-96-Al / GO, the temperature of the hydrothermal reaction is 100-150° C., and the time is 6-12 hours.

8. A method for preparing a lithium ion battery fire extinguishing agent as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: The MIL-96-Al / GO and perfluorohexanone are mixed, stirred, and then ultrasonically treated to obtain the lithium-ion battery fire extinguishing agent.

9. The method for preparing a lithium ion battery fire extinguishing agent according to claim 8, characterized in that: The stirring is performed at room temperature; the stirring time is greater than or equal to 6 hours.

10. The method for preparing a lithium ion battery fire extinguishing agent according to claim 8 or 9, characterized in that: The ultrasonic treatment time is 1 to 3 hours, and the temperature does not exceed 30°C.

Citation Information

Patent Citations

  • Novel insulating anti-corrosion fire extinguishing agent and preparation method thereof

    CN113209537A

  • Low-boiling-point slow-release cooling fire extinguishing agent as well as preparation method and application thereof

    CN117504216A

  • Flame-retardant fire-extinguishing material MILQIJ-1230, preparation method thereof, fire-extinguishing flame-retardant patch and application of fire-extinguishing flame-retardant patch

    CN118001671A

  • Lithium ion battery compound fire extinguishing agent and preparation method and application thereof

    CN119327079A

  • Sulfonated cellulose, proton conducting polymer membranes using the same, and polymer electrolyte membrane fuel cell having proton conducting polymer membranes

    KR1020180107544A

Cited By

  • Lithium battery fire extinguishing agent, preparation method thereof and fire extinguisher

    CN119548788A