Low-grade attapulgite and coal gasification ash based geopolymer film as well as preparation method and application thereof

The geological polymerization technology of low-grade concave and concave rock stone and gasified ash slag prepared without sintering, which solved the high energy consumption and high cost problems caused by high temperature sintering of traditional inorganic membranes, achieved efficient removal of PM2.5, and reduced production Cost and energy consumption.

CN118988004APending Publication Date: 2024-11-22HUAIYIN TEACHERS COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410737580.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

High temperature sintering during the preparation of traditional inorganic films leads to high energy consumption and high cost, and the removal rate of PM2.5 is low, which cannot meet the strict exhaust emission requirements.

Method used

Using low-grade concave and convex rock stone and gasified ash slag as raw materials, geological polymer films without sintering are prepared through geological polymerization technology, the compound ratio, exciter modulus, alkali parameter, water-cement ratio and curing time are adjusted, and peroxidation is introduced Hydrogen regulates the pore structure to prepare a geological polymer film of concave-concave-coal gasified ash slag base with excellent mechanical properties and gas-solid separation properties.

Benefits of technology

Achieve film preparation without sintering, low cost, cost about 11.82 ¥/m2, low energy consumption, excellent mechanical properties and gas-solid separation performance, the removal rate of PM2.5 in flue gas reaches more than 90%, and has good separation performance .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988004A_ABST
    Figure CN118988004A_ABST
Patent Text Reader

Abstract

The invention discloses a geopolymer film based on low-grade attapulgite and coal gasification ash and a preparation method and application thereof.The preparation method comprises the following steps that after low-grade attapulgite and coal gasification ash are mixed, an exciting agent and water are added, the mixture is stirred to be uniform, and a geopolymer is obtained; and uniformly mixing the geopolymer with H2O2 and lauryl sodium sulfate, casting, defoaming and maintaining to obtain the geopolymer membrane. When the mass ratio of the attapulgite to the coal gasification ash is 1: 5, the modulus of the excitant is 1.5, the water-cement ratio is 0.5, the alkali doping amount is 10% and the curing time is 28 days, the geopolymer membrane with the compressive strength of 16.9 MPa and the gas flux of 1101 L / m < 2 > / h / bar can be prepared, the average pore diameter of the geopolymer membrane is 28.3 microns, the particle rejection rate is greater than 90% when dust-containing waste gas is treated, and the geopolymer membrane shows excellent separation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-grade attapulgite and coal gasification ash-based geopolymer membrane and a preparation method and application thereof, belonging to the technical field of membrane preparation and separation. Background Art

[0002] The rapid development of industrial processes has led to increasingly serious environmental pollution, which not only seriously affects air quality, but also endangers human health. Strictly controlling the emission of ultrafine dust in industrial exhaust gas and achieving efficient and clean utilization of resources are key issues facing the fields of chemical industry and energy. Therefore, the development of separation technology for gas dust removal is of great significance. At present, traditional gas dust removal methods mainly include electrostatic dust removal, cyclone separation and bag dust removal. After years of development, these technologies have achieved large-scale industrial applications. However, for the fine particulate matter (PM2.5) newly discovered in the gas in the past decade, due to its special micro-nano size, the traditional dust removal method has a low PM2.5 removal rate and cannot meet the strict exhaust emission requirements. At present, the air filter material has low precision and high resistance. Membrane separation technology has the advantages of high separation precision and low process energy consumption. In recent years, it has been widely studied in the field of gas dust removal and provides an effective way to control PM2.5. Among them, inorganic membranes have shown good application prospects in gas dust removal, especially in the purification process of high-temperature gas, due to their stable chemical properties, high mechanical strength and long service life, and have become one of the best choices for gas purification.

[0003] Inorganic membranes have excellent performance in gas purification, but their high cost seriously restricts their promotion and application. Inorganic membranes are mainly made of inorganic oxides, and commonly used raw materials are Al2O3, SiO2, TiO2, ZrO2, etc. and their composites. At present, commercial inorganic membranes are made of high-purity inorganic oxides. The high cost of raw materials is a major reason for the high cost of membranes. Studies have shown that the use of cheap raw materials such as minerals and industrial waste to prepare inorganic membranes can reduce membrane costs by about 30%. Materials such as kaolin, cordierite, fly ash, and attapulgite clay, whose main components are SiO2 and Al2O3, are commonly used raw materials for the preparation of commercial inorganic membranes, and therefore are also used by researchers to prepare low-cost inorganic membranes.

[0004] Suresh et al. used fly ash as raw material and prepared a ceramic microfiltration membrane for oil-water separation by sintering at 1100℃. The porosity was as high as 43% and the retention rate was 81-99%. Fan et al. used attapulgite clay as the main raw material and prepared a ceramic membrane support based on low-grade attapulgite clay after sintering at 700℃. The performance was the best, with an average mechanical strength of (17.76±2.03)MPa and a porosity of (44±0.3)%. Among them, a large amount of low-grade attapulgite tailings will be produced during the mining of nano-attapulgite. The tailings are discharged at will, causing waste of resources and environmental pollution. Therefore, the preparation of inorganic membranes with attapulgite tailings not only solves the problem of high cost of inorganic membrane preparation, but also realizes the economic utilization of tailings.

[0005] Although the use of cheap raw materials, such as low-grade ATP, to prepare inorganic membranes reduces the cost of the membranes to a certain extent, it still requires high-temperature sintering to form them, and the sintering temperature is often above 700°C. The high-temperature sintering of inorganic membranes is a high-energy consumption process, and its sintering energy consumption accounts for about 60% of the total cost of membrane production, which is another reason for the high cost of membrane preparation. Therefore, the difficulty in developing inorganic membrane preparation technology based on low-grade attapulgite is to solve the high cost problem caused by the high energy consumption in the preparation process.

[0006] Geopolymer is an inorganic material with amorphous and quasi-crystalline characteristics formed by the polymerization of silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron. It has the advantages of excellent mechanical properties, acid and alkali resistance, high temperature resistance, etc., and it can be formed at low temperature without sintering, and has the characteristics of low energy consumption and low cost. Therefore, the preparation of inorganic membranes by geopolymerization technology can overcome the high energy consumption problem caused by the high-temperature sintering process of traditional inorganic membranes, and is expected to significantly reduce the cost of inorganic membranes. The raw materials of geopolymers are widely available, and can be artificially synthesized silica-aluminide, aluminosilicate minerals such as kaolin, and solid waste containing silicon components. By stimulating the silicon-aluminum material in the raw material, the internal Si-O tetrahedron and Al-O tetrahedron are connected by sharing O to form a geopolymer with mechanical strength.

[0007] At present, the main raw material used to prepare geopolymers is metakaolin. Zhang et al. reported a geopolymer membrane based on metakaolin, which has a mechanical strength of 14 MPa, a porosity of about 70%, and a water flux of 100-8000 kg·m -2 ·h -1 (25℃, 1MPa), the removal rate of PM2.5 in flue gas is as high as 97%, and particles with a particle size greater than 1.67μm in carbon black aqueous solution can be captured. The content of SiO2 and Al2O3 in low-grade attapulgite tailings accounts for more than 70%, which has the material basis for the preparation of geopolymer inorganic membranes and is also a potential raw material for the preparation of geopolymer membranes. However, no related research has been reported. Summary of the invention

[0008] The purpose of the present invention is to provide a low-grade attapulgite and coal gasification ash-based geopolymer membrane and its preparation method and application, and to reduce production costs and energy consumption from the source by adopting low-energy consumption geopolymer preparation technology to replace the traditional high-temperature sintering process to prepare inorganic membranes. Low-grade ATP is used as a raw material, and geopolymer is prepared by introducing coal gasification ash to prepare geopolymer, and by adjusting the compounding ratio, activator modulus, alkali parameters, water-cement ratio, curing time, etc., a geopolymer membrane with excellent mechanical properties and phase structure is obtained, and by introducing hydrogen peroxide to adjust the pore structure of the geopolymer, an attapulgite-coal gasification ash-based geopolymer membrane (AGM) with connected pores is obtained, and the membrane has excellent gas-solid separation performance.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] A method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane comprises the following steps:

[0011] After mixing low-grade attapulgite and coal gasification ash, an activator and water are added, and the mixture is stirred evenly to obtain a geopolymer; the geopolymer is then mixed evenly with H2O2 and sodium dodecyl sulfate, and the geopolymer film is obtained through casting, defoaming and curing;

[0012] The mass ratio of low-grade attapulgite to coal gasification ash is 1:(3-8); and the activator is sodium water glass with a modulus of 1.0-2.0.

[0013] Preferably, the ratio of the amount of water added to the total mass of the low-grade attapulgite and the coal gasification ash is 0.3-0.8.

[0014] Preferably, the activator is prepared by adding NaOH to industrial sodium water glass to adjust the modulus to 1.0-2.0.

[0015] Preferably, the alkali content in the activator is 5-15% of the total mass of the low-grade attapulgite and the coal gasification ash, calculated on a Na2O equivalent basis.

[0016] Preferably, the amount of H2O2 added is 3-7% of the mass of the geopolymer.

[0017] Preferably, the amount of sodium lauryl sulfate added is 5-15% of the amount of H2O2 added.

[0018] Preferably, the geopolymer is first stirred with H2O2 at 500-1000 rpm for 2-5 min, then stirred at 1500-3000 rpm for 2-5 min, and then sodium dodecyl sulfate is added; after adding sodium dodecyl sulfate, it is stirred at 1500-3000 rpm for 2-5 min.

[0019] Preferably, the curing is carried out at room temperature for 1-30 days.

[0020] A low-grade attapulgite and coal gasification ash-based geopolymer membrane is prepared by any of the above methods.

[0021] The application of the above-mentioned low-grade attapulgite and coal gasification ash-based geopolymer membrane in gas-solid separation of dust-containing waste gas.

[0022] The beneficial effects of the present invention are:

[0023] 1. No need for sintering, low cost. The preparation cost of AGM is about 11.82¥ / m 2 , which is much lower than that of inorganic membranes prepared by high-temperature sintering, and has the advantages of low cost, low energy consumption, simple process, and green environmental protection;

[0024] 2. Excellent mechanical properties and gas-solid separation performance. When the mass ratio of attapulgite to coal gasification ash is 1:5, the modulus of the activator is 1.5, the water-cement ratio is 0.5, the alkali content is 10%, and the curing time is 28 days, the synthesis performance of AGM is the best. When the H2O2 content is 6%, the pore size of AGM is 28.3μm, the compressive strength is 16.9MPa, and the removal rate of PM2.5 / 10 in flue gas is above 90%, with good separation performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a flow chart for the preparation of geopolymer membranes;

[0026] Figure 2 is the compressive strength of geopolymer at different modulus and water-cement ratio;

[0027] Figure 3 (a) XRD of geopolymer under different activator modulus; (b) FT-IR of geopolymer under different activator modulus;

[0028] Figure 4 (ac) surface structure of samples with modulus 1.0, 1.5, and 2.0; (df) cross-sectional structure of samples with modulus 1.0, 1.5, and 2.0;

[0029] Figure 5 (a) The compressive strength of geopolymers at different slag contents; (b) The compressive strength of geopolymers at different alkali contents;

[0030] Figure 6 (a) FT-IR of geopolymers at different slag contents; (b) XRD of geopolymers at different slag contents; (c) TG of geopolymers at different slag contents;

[0031] Figure 7(aj) The cross-sectional morphology of AG-Slag with different proportions when the alkali content is 10%;

[0032] Figure 8 is the compressive strength of geopolymer under different curing times;

[0033] Fig. 9 (ae) Surface structure of samples with 3% to 7% H2O2 addition; (fj) Cross-sectional structure of samples with 3% to 7% H2O2 addition;

[0034] Fig.10 (ae) The cross-sectional structure of the sample with H2O2 addition of 3% to 7%;

[0035] Fig.11 (a) The effect of H2O2 addition on the pore size distribution of AGM; (b) The effect of H2O2 addition on the porosity of AGM;

[0036] Fig.12 is the compressive strength of AGM under different H2O2 addition amounts;

[0037] Fig.13 (a) The filtration effect of AGM on PM2.5 / 10 under different H2O2 addition amounts; (b) The permeation flux of N2 through AGM under different H2O2 addition amounts. DETAILED DESCRIPTION

[0038] The present invention will be specifically described below in conjunction with the accompanying drawings and embodiments.

[0039] The present invention uses low-grade and cheap attapulgite and coal gasification ash as the main raw materials, and combines geopolymerization technology to prepare a sinter-free low-cost attapulgite-coal gasification ash geopolymer membrane. The effects of different attapulgite and coal gasification ash ratios, modulus, water-cement ratio, alkali content, curing time and other parameters on the performance of the geopolymer membrane are investigated, and the specific contents are as follows.

[0040] Experimental materials and reagents

[0041] The invention uses ATP and coal gasification ash as main raw materials to prepare geopolymer, and the chemical composition of the raw materials is determined by X-ray fluorescence (XRF). ATP is produced in Inner Mongolia Autonomous Region of China, and mainly contains 49.875% of SiO2 and 17.065% of Al2O3. Coal gasification ash mainly contains 56.979% of CO2, 15.858% of SiO2, 8.256% of CaO and 7.233% of Al2O3. The activator is prepared from sodium hydroxide (NaOH, 96.0%) and industrial sodium water glass (Na-WG, modulus: n(SiO2) / n(Na2O)=3.3, water content 65.2%), and the modulus is adjusted by adding NaOH to the sodium water glass. Hydrogen peroxide (H2O2, 30%) and sodium dodecyl sulfate are used as foaming (pore-forming) agent and bubble stabilizer respectively to adjust the pore size of the geopolymer film.

[0042] Preparation of porous geopolymers

[0043] Adding coal gasification ash can promote further hydration of geopolymer, generate CSH gel, improve the microstructure of AGM, and make contact with water glass more fully, thereby changing the mechanical properties of AGM. Different compositions of attapulgite, coal gasification ash, activator (compound of industrial sodium water glass and NaOH) and water were prepared in batches. Low-grade attapulgite and coal gasification ash from Inner Mongolia Autonomous Region were used to prepare geopolymers (AG-Slag) of different compositions. Solid AG-Slag was mixed with composite alkali activator (sodium dodecyl sulfate, added in an amount of 10% of H2O2 addition), stirred at 800 rpm for 2 min in a mixer, then stirred at 2200 rpm for 2 min, and finally, a foaming agent (H2O2) was added and stirred at 2200 rpm for 2 min, and then the slurry was cast into a cylindrical sheet mold (size 30*2 mm). After eliminating bubbles with a vibrator, the geopolymer membrane samples were placed in a room temperature room for curing for 1, 3, 7, 14 and 28 days, and then characterization tests and compressive strength tests were performed. Figure 1 shown.

[0044] Characterization methods

[0045] X-ray powder diffraction (MiniFlex600, Rigaku, Japan) was used for phase analysis and characterization of AGM crystallinity. The microstructure of AGM with different ratios was observed by scanning electron microscopy (QuantaFEG450, FEI, USA). Fourier transform infrared (AVATAR360, Nicoli, USA) was used to test the spectral range from 4000 to 400 cm -1For molecular structure analysis. The mechanical properties of AGM were determined by electronic universal pressure testing machine (Shimadzu Japan). TG (TGA-STA449F3, Netzsch, GER) was used to characterize the temperature-mass change relationship of geopolymer. The pore size distribution and porosity were analyzed using a pore size analyzer (PSDA-20, Nanjing Gaoqian Functional Materials Technology Co., Ltd., China).

[0046] Effects of activator modulus (Ms) and water-cement ratio on mechanical properties and microstructure of geopolymers

[0047] The universal testing machine tests the compressive strength of geopolymers with different modulus and water-cement ratios. Figure 2 As shown, it can be observed that the geopolymer made of attapulgite and coal gasification ash from Inner Mongolia Autonomous Region has the highest strength when the modulus of the activator is 1.5 and the water-cement ratio is 0.5. When the modulus of water glass is 1.0, the OH- content in the alkaline activator is the highest and the alkalinity is the strongest, but [SiO4] 4- The content is the lowest, affecting [SiO4] 4- With Ca 2+ The amount of CSH and CASH gel produced by the reaction makes [SiO4] 4- With Ca 2+ The amount of CSH and CASH gel generated by the reaction is relatively small, which affects the compressive strength of the specimen. As the modulus of water glass increases, [SiO4] 4- The content of water glass continues to increase, which makes the cementitious material hydrated to produce more CSH and CASH gel, thereby improving the compressive strength of the alkali-activated coal gasification ash cementitious material; with the continuous increase of the water glass modulus, the alkalinity of the alkali activator decreases, and the activation effect on the coal gasification ash weakens, causing the compressive strength of the cementitious material to decrease. The compressive strength increases first and then decreases with the increase of water-cement ratio. This is because when the water-cement ratio is small, it will affect the secondary dissolution and polycondensation process of ATP and coal gasification ash, while when the water-cement ratio is too large, the OH in the reaction system will - The concentration decreases, and the SiO4 2- The solubility decreases, making [SiO4] 4- and [AlO4] 5- The polycondensation reaction of oligomers becomes more difficult to proceed to the direction of polymers, and it is even more difficult to develop into the crystal phase, resulting in a decrease in the compressive strength of the sample. In summary, as the water glass modulus and water-cement ratio increase, the compressive strength of the cementitious material increases first and then decreases.

[0048] like Figure 3As shown in the a region, the prepared sample has an X-ray diffraction spectrum similar to that of the attapulgite raw material, with almost no disappearance or increase of any characteristic peaks and changes in intensity, which indicates that no new crystalline phase is generated in the sample reaction, and an amorphous dispersion peak is formed between 20 and 40° at 2θ, which belongs to an amorphous structure. Figure 3 It can be seen from the middle b area that different moduli have little effect on the chemical composition of geopolymers. -1 The main broad absorption band is shown at 785 cm-1, and the corresponding characteristic peak is the asymmetric stretching vibration of Si-O-Si. -1 The corresponding characteristic peak is the asymmetric stretching vibration of Si-O-Al.

[0049] Geopolymer samples were collected through compressive strength test and the microstructure of the samples was observed using scanning electron microscopy. Figure 4 In the middle ac region, the surface micromorphology of the prepared geopolymer ceramics was characterized. The influence of activators with different moduli on the morphology of geopolymer ceramics was investigated. From the figure, it can be seen that when the modulus of activators with different moduli is added, the degree of geopolymerization of the sample is the best, the surface is flat and there are fewer cracks. Figure 4 In the middle df region, it was found that the microstructure of the cross section of the geopolymer prepared with different water glass modulus was not much different. They were all composed of gel generated by geopolymerization reaction and the overall structure was compact. However, by comparing the SEM images of the three groups, it was found that the structure of the test group with the activator modulus of 1.5 had less powder particles, indicating that its degree of polymerization was higher. This is due to the large amount of OH in the alkaline activator. - The ions will destroy the -Si-O-, -Al-O- and other bonds in attapulgite, causing the internal structure of attapulgite to decompose, activating the silicon-aluminum material, and Ca in attapulgite 2+ 、SiO4 4- Plasma dissolution provides counter cations during the geopolymerization process. However, samples with the same modulus activator show cracks as the alkali dosage increases. This is because during the polymerization process, water loss causes alkali precipitation, and the crystal structure formed produces stress in the ceramic, thereby generating cracks.

[0050] Effects of alkali and slag content on mechanical properties and microstructure of geopolymers

[0051] The modulus of the activator was determined to be 1.5 and the water-cement ratio was 0.5 to prepare the geopolymer. On this basis, the effects of alkali content, slag content and curing time on the strength of the geopolymer were further studied. Figure 5It can be seen from the a and b areas that the mass ratio of ATP to coal gasification ash is 1:5, and when the alkali content is 10% (calculated as Na2O equivalent), the mechanical properties of the geopolymer are the best. This is because the slag is a high-calcium system, and the Ca-O bond in the slag skeleton is much weaker than the Al-O and Si-O bonds, and is easier to break in an alkaline solution. The calcium in the coal gasification ash can promote the aluminosilicate reaction. When the activator content is low, the alkaline environment provides insufficient conditions, and OH - When the concentration is low, the hydrolysis effect on the raw materials is weak; when the dosage of the alkaline activator is too high, a large amount of gel products are generated in a short time, which is easy to wrap the coal gasification ash and attapulgite raw material particles, affecting the full contact between the silica-alumina raw material and the liquid alkaline activator, making [SiO4] 4- 、[AlO4] 4- and Ca 2+ The reduction in the amount of ion dissolution will affect the continued increase in the amount of polymerization products in the later stage of the reaction. Therefore, there is an optimal value for the dosage of the base activator, and the more the better is not necessarily true.

[0052] FT-IR spectrum of geopolymers Figure 6 As shown in the a region, at 1650 and 3650 cm -1 The peaks appearing around 1400-1450cm correspond to the vibration peaks of -OH bonds. -1 The peak at 2θ corresponds to the vibration peak of C=O bond. This is because geopolymer needs alkali activation, which makes geopolymer contain high alkali and easily react with CO2 in the air to form carbonate. Geopolymers with different slag content all have amorphous dispersion peaks at 2θ=20-40° ( Figure 6 Area b in the middle), which is a typical amorphous aluminosilicate. SiO2 diffraction peaks appeared at 2θ=21, 27°, etc. With the increase of the amount of coal gasification ash, the intensity of the SiO2 diffraction peak became weaker and weaker, indicating that the addition of slag helps SiO2 participate in the geopolymerization reaction. The XRD patterns of samples with different compounding ratios are similar, but the compressive strengths vary greatly. This is due to the different degrees of polymerization. The higher the content of active alumina in the mixture, the greater the degree of polymerization, the higher the compressive strength of the sample, and the faster the compressive strength increases. Thermogravimetric (TG) analysis of geopolymers at different slag dosages is shown in the figure. Figure 6 As shown in the middle c area. The mass of the geopolymer drops sharply below 200°C, which means that the weight loss area of ​​the sample is mainly related to the evaporation of free water. The mass loss rate decreases after 200°C, which is due to the dissipation of bound water. Before 150°C, the geopolymer loses weight at the fastest rate. Due to the particularity of its pore structure, the excess free water evaporates quickly, and there is basically no mass change after 700°C. This is the thermal stability zone of the geopolymer, indicating that it has good thermal stability.

[0053] exist Figure 7In the middle ae region, the geopolymer structure becomes relatively dense with the increase of coal gasification ash content. This is due to the generation of more CASH / CSH gel. The microstructure observed by SEM corresponds to the above compressive strength.

[0054] Effect of curing time on compressive strength of geopolymers

[0055] Figure 8 The compressive strength values ​​of geopolymers measured during different curing periods show that the compressive strength of the sample can reach 10.02MPa during the 1d curing period. Combined with the XRD graph, the rapid increase in sample strength is due to the polymerization reaction of silicon and aluminum in the sample, which makes the sample have the characteristics of early strength and fast hardening. Comparing the compressive strength values ​​of the samples during different curing periods, it can be seen that the compressive strength of geopolymers increases to a certain extent with the increase of curing time. During the 28d curing period, the compressive strength has reached 20.96MPa.

[0056] Effect of H2O2 addition on the microstructure of AGM

[0057] The microstructure of AGM is as follows Fig. 9 As shown, it can be seen that the surface of AGM contains almost no pores. This is because the surface is affected by surface tension during standing at room temperature, causing most of the pores to be closed. In addition, there are a large number of incompletely reacted particles on the surface. This is because during standing at room temperature, as the slurry foams and expands to above the mold groove, the surface raw materials are exposed to less alkali solution. Incompletely reacted particles can easily detach from the upper surface and enter the internal pores, causing blockage of the pores. In contrast, the bubbles in the internal pores grow more fully during the formation process, thus forming larger pores. Overall, the internal structure of porous geopolymers is similar to that of ceramic membrane filter materials.

[0058] In order to study the changes in the microstructure of the internal pore structure of AGM with the addition of H2O2, SEM observations were performed on AGM with different H2O2 additions. The results are shown in Figure 2. Fig.10 As shown. Fig.10 It can be seen from the middle ae area that when the amount of H2O2 added is 3%, 4% and 5%, the interior is mostly closed pores with uneven pore size; when the amount of H2O2 added is 6%, uniform through pores are formed inside with obvious pore walls; when the amount of H2O2 added increases to 7%, the pore size becomes larger, the pore wall gradually becomes thinner, and the structure becomes loose. This change is due to the fact that the foam stabilizer can retain most of the foam during the pore formation period. As the gas generated by the decomposition of H2O2 increases, the foam is more likely to merge to form larger bubbles, which increases the pore size of the porous geopolymer. Therefore, the amount of H2O2 added has a great influence on the pore structure of the porous geopolymer.

[0059] Effect of H2O2 addition on the porosity of AGM

[0060] The filter material needs to have a suitable pore structure. Since there are macropores, mesopores and micropores in AGM, the function of macropores is mainly to increase the water flux and porosity of AGM, and the main function of mesopores is to filter materials with smaller particle sizes. To this end, the present invention tests the effect of H2O2 addition on the pore size distribution and porosity of AGM. When the H2O2 addition amount is 3%, 4%, 5%, 6% and 7% respectively, the average pore size gradually increases with the addition amount of H2O2. When the addition amount is 6%, the average pore size reaches 28.3μm. Fig.11 The middle b area shows the effect of H2O2 addition on the porosity of AGM, indicating that the porosities corresponding to the five H2O2 additions are 49%, 55%, 64%, 70% and 80%, respectively. These changes are caused by the increase in the foaming ability of H2O2 as the addition amount increases. It can be seen that when the H2O2 addition amount is 6%, the average pore size and pore size distribution range of AGM are most moderate, and the porosity is high, showing a good pore structure.

[0061] Effect of H2O2 addition on compressive strength of AGM

[0062] The smoke filter material will be subjected to certain external stress during use, and high requirements are placed on its mechanical properties. The present invention tests the changes in the compressive strength of AGM with different H2O2 addition amounts. The results are as follows: Fig.12 At room temperature, when the amount of H2O2 added was 3%, 4%, 5%, 6% and 7%, the compressive strength of AGM with a curing time of 28 days was 20.26, 18.91, 17.59, 16.9 and 13.2 MPa, respectively, showing a clear downward trend. Fig.10 The pore morphology analysis shows that with the increase of H2O2 addition, the structure of the porous geopolymer becomes loose, resulting in a gradual decrease in the compressive strength of the AGM. This is because with the increase of H2O2 addition, more foam is generated in the reaction system within a limited space, and the open porosity is larger, which is related to Fig.10 Therefore, appropriately reducing the amount of H2O2 added is beneficial to maintaining the compressive strength of AGM.

[0063] Application of AGM in gas-solid separation

[0064] In order to characterize the filtration performance of AGM, its filtration efficiency was tested and the results are as follows: Fig.13 shown. Fig.13Area a in the middle shows the effect of H2O2 addition on filtration performance. When the H2O2 addition was 3%, 4%, 5%, 6% and 7%, the filtration efficiency of porous geopolymer for PM10 and PM2.5 was 99.1%, 98.5%, 96.4%, 95.1%, 92.2% and 98.3%, 96.9%, 94.2%, 91.8%, 86.7%, respectively. Fig.11 From the pore size distribution in the middle a region, it can be seen that with the increase of H2O2, the average pore size increases, making it easier for particles to penetrate the AGM with the airflow, thus reducing the interception effect on the flue gas. Fig.13 As can be seen from the middle b area, the permeation flux of N2 through AGM increases with the increase of H2O2 addition. Fig.11 The change in porosity in region b shows that the increase in AGM porosity increases the flux. Therefore, when the H2O2 addition amount is 6%, AGM has the most suitable filtration efficiency and flux.

[0065] In summary, the present invention combines geopolymerization technology to prepare a non-sintered, low-cost AGM at room temperature and pressure. The raw material price of AGM is about 0.0334 ¥ (mold size: bottom diameter 300mm, height 2.5mm), and the preparation cost is about 11.82 ¥ / m 2 , which is much lower than the inorganic membrane prepared by high-temperature sintering. It has the advantages of low cost, low energy consumption, simple process, green environmental protection, and excellent mechanical properties. And when the mass ratio of attapulgite to coal gasification ash is 1:5, the modulus of the activator is 1.5, the water-cement ratio is 0.5, the alkali content is 10%, and the curing time is 28d, the synthesis performance of AGM is the best. When the H2O2 content is 6%, the pore size of AGM is 28.3μm, the compressive strength is 16.9MPa, and the removal rate of PM2.5 / 10 in flue gas is above 90%, with good separation performance.

[0066] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the scope of protection of the patent of the present invention.

Claims

1. A method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane, characterized in that: The steps include: After mixing low-grade attapulgite and coal gasification ash, an activator and water are added, and the mixture is stirred evenly to obtain a geopolymer; the geopolymer is then mixed evenly with H2O2 and sodium dodecyl sulfate, and the geopolymer film is obtained through casting, defoaming and curing; The mass ratio of low-grade attapulgite to coal gasification ash is 1:(3-8); and the activator is sodium water glass with a modulus of 1.0-2.

0.

2. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: The ratio of the amount of water added to the total mass of the low-grade attapulgite and the coal gasification ash is 0.3-0.

8.

3. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: The activator is prepared by adding NaOH to industrial sodium water glass to adjust the modulus to 1.0-2.

0.

4. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: Calculated in terms of Na2O equivalent, the alkali content in the activator is 5-15% of the total mass of the low-grade attapulgite and the coal gasification ash.

5. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: The amount of H2O2 added is 3-7% of the mass of the geopolymer.

6. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: The amount of sodium lauryl sulfate added is 5-15% of the amount of H2O2 added.

7. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: The geopolymer is first stirred with H2O2 at 500-1000 rpm for 2-5 min, and then stirred at 1500-3000 rpm for 2-5 min before adding sodium dodecyl sulfate; after adding sodium dodecyl sulfate, it is stirred at 1500-3000 rpm for 2-5 min.

8. The method for preparing a low-grade attapulgite and coal gasification ash-based geopolymer membrane according to claim 1, characterized in that: Curing is carried out at room temperature and the curing time is 1-30 days.

9. A low-grade attapulgite and coal gasification ash-based geopolymer membrane, characterized in that: The method is prepared by any one of claims 1 to 8.