Preparation method and application of super-hydrophobic cobalt ferrite

The preparation of superhydrophobic cobalt ferrite through co-precipitation method and surface modification has solved the problems of low efficiency and high cost of microplastic removal and water-oil separation in the prior art, and achieved efficient and environmentally friendly microplastic removal and water-oil separation. And the material is renewable.

CN118988243AInactive Publication Date: 2024-11-22NANJING AGRICULTURAL UNIVERSITY

Patent Information

Application Number
CN202411480275.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has problems such as long-term process, complex operation, high cost, and water pollution caused by the use of toxic reagents in removing microplastics and water-oil separation, and there are few researches on the functionalization of magnetic nanoparticles.

Method used

The superhydrophobic cobalt ferrite was prepared by co-precipitation method, and it was functionalized by lauric acid surface modification to make it stable hydrophobicity and magnetic properties. It was recycled by permanent magnets, and it was efficiently adsorbed and separated under different microplastic concentrations. Water and oil.

Benefits of technology

The removal efficiency of microplastics is achieved by nearly 100% and the separation efficiency of water and oil is higher than 94%, while avoiding the use of toxic reagents, reducing the surface energy and roughness of the material, and having the advantages of renewable and reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988243A_ABST
    Figure CN118988243A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of super-hydrophobic cobalt ferrite, and the preparation method comprises the following steps: step 1, mixing a FeCl3. 6H2O solution and a CoCl2. 6H2O solution to obtain a mixed solution; 2, sequentially adding octanoic acid and a NaOH solution into the mixed solution; and 3, stirring, cooling, washing, drying and carrying out heat treatment on the solution in the step 2 to obtain the cobalt ferrite. 4, lauric acid is dissolved in absolute ethyl alcohol, and a modified solution is obtained. Step 5, adding cobalt ferrite into the modified solution, placing at room temperature for a first time, and absorbing the modified solution by using a magnet; and washing and airing the cobalt ferrite after reaction to obtain the super-hydrophobic cobalt ferrite. According to the preparation method, on the basis of a coprecipitation method and surface modification, lauric acid is adsorbed on the surface of cobalt ferrite, the cobalt ferrite is subjected to surface modification, the super-hydrophobic cobalt ferrite with stable hydrophobicity and magnetism is generated, the efficiency of the super-hydrophobic cobalt ferrite for removing micro-plastics is high, and oil-water separation can be well achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation and wastewater treatment, and in particular to a preparation method and application of super-hydrophobic cobalt ferrite. Background Art

[0002] Plastic fragments with a diameter of less than 5 mm are defined as microplastics, which have attracted widespread attention due to their potential adverse effects on organisms. Due to the large specific surface area of ​​microplastics, heavy metals and persistent organic pollutants easily adhere to and accumulate on the surface of microplastics, and then migrate in the environment. Microplastics are easily absorbed by marine organisms and enter the food chain, thus posing a threat to public health. The human body is exposed to microplastics through food and drinking water, and microplastics have an impact on the human body. The hazards caused by microplastics highlight the need to separate them from the environment. In recent years, people have adopted various methods and technologies to remove microplastics. For example, wastewater plants use membrane filtration, adsorption, coagulation, agglomeration, biodegradation and photocatalysis to treat sewage. The above strategies for removing microplastics have the disadvantages of time-consuming processes, complex operations, high costs and difficulty in large-scale production. In addition, in actual application scenarios, water environments often face more complex problems, including organic and oil pollution.

[0003] In recent years, the use of magnetic materials to replace filtration or multi-stage treatment to remove microplastics and other pollutants in water has received widespread attention. Magnetic materials have the advantages of being renewable and reusable, and can minimize the generation of hazardous waste. Cobalt ferrite (CoFe2O4) is a material with high magnetocrystalline anisotropy, high coercivity and moderate magnetization. Nanospinel ferrite has attracted attention due to its small particle size, narrow particle size distribution and large surface area. Several methods for synthesizing cobalt ferrite have been developed, including hydrothermal method, sol-gel method, chemical reduction method, microwave synthesis method, mechanical alloying method and coprecipitation method. Among these methods, coprecipitation method has the advantages of low toxicity, rapid preparation and low cost.

[0004] Studies have shown that the efficiency of microplastic removal is related to surface wettability and wetting stability. Materials with low surface roughness and low surface energy have strong water repellency and oil absorption capabilities, and show high efficiency in treating oily wastewater pollution. In order to achieve long-term separation and improve separation performance, it is necessary to reduce the surface roughness and surface energy of the material to achieve a superhydrophobic state. Therefore, it is urgent to study the functionalization of magnetic nanoparticles (MNPs). Saturated fatty acids have the characteristics of regulating wettability by adjusting surface groups. Low-cost lauric acid, as a low-surface-energy fatty acid, can dehydrate with the surface hydroxyl groups of nanomaterials, and the long carbon chain is distributed on the surface of nanomaterials to reduce their surface energy to achieve superhydrophobic properties. The existing technology uses lauric acid-modified superhydrophobic cellulose composite membranes for oil-water separation. However, there is little research on the removal of pollutants such as microplastics by functionalizing magnetic nanoparticles by modifying magnetic nanoparticles with lauric acid.

[0005] Patent No. CN116143218B discloses a method for removing microplastics from water medium based on bubble flotation, which adds N,N-di(hexadecyl)-N-methyl-1-hexadecyl ammonium chloride to water containing microplastics, and the pH value needs to be adjusted to achieve the removal of microplastics. The reagents added in this method are highly toxic and will destroy the living environment of aquatic organisms, have long-term and lasting effects, and cause secondary pollution of water bodies. Summary of the invention

[0006] To overcome the problems in the related art, one of the objects of the present invention is to provide a method for preparing a super hydrophobic cobalt ferrite, the method uses magnetically functionalized cobalt ferrite particles to remove microplastics and organic pollutants from water, based on a coprecipitation method and surface modification, lauric acid is adsorbed on the surface of cobalt ferrite to produce cobalt ferrite particles with stable hydrophobicity and magnetism. Super hydrophobic cobalt ferrite can be recovered using a permanent magnet. The present invention has tested super hydrophobic cobalt ferrite, proving that super hydrophobic cobalt ferrite has good effects in removing microplastics and water-oil separation.

[0007] A method for preparing super-hydrophobic cobalt ferrite comprises the following steps: Step 1: Mixing FeCl3.6H2O solution and CoCl2.6H2O solution to obtain a mixed solution; Step 2: adding octanoic acid and NaOH solution to the mixed solution in sequence; Step 3: stirring, cooling, rinsing, drying and heat treating the solution in step 2 to obtain cobalt ferrite; Step 4: dissolving lauric acid in anhydrous ethanol to obtain a modified solution; Step 5: adding the cobalt ferrite to the modified solution, leaving it at room temperature for a first period of time, and using a magnet to absorb the modified solution; rinsing and drying the cobalt ferrite after the reaction to obtain superhydrophobic cobalt ferrite.

[0008] In a preferred technical solution of the present invention, the modified solution in step 4 is obtained by dissolving 0.5 g of lauric acid in 5 ml of anhydrous ethanol.

[0009] In a preferred technical solution of the present invention, the concentration of the FeCl3.6H2O solution in step 1 is 0.4 mol / L, the concentration of the CoCl2.6H2O solution is 0.2 mol / L, and the volumes of the FeCl3.6H2O solution and the CoCl2.6H2O solution are both 25 ml.

[0010] In a preferred technical solution of the present invention, the volume of octanoic acid in step 2 is 0.1-2 ml, and the concentration of the NaOH solution is 1.5 mol / L.

[0011] In a preferred technical solution of the present invention, the pH value of the solution in step 2 is 7.5-8 In the preferred technical solution of the present invention, the stirring time in step 3 is 1 hour, the stirring temperature is 80°C; the centrifugal time is 2 minutes, the centrifugal speed is 1500 rpm; the drying temperature is 80°C, the drying time is 8 hours; the heat treatment time is 1 hour, the heat treatment temperature is 900°C The second object of the present invention is to provide an application of super-hydrophobic cobalt ferrite in the removal of microplastics, including: Step a: Take 5 ml of water and place it in a container, then add different amounts of microplastics; Step b: stirring the water and microplastics in the container; Step c: placing the super hydrophobic cobalt ferrite into the container; Step d: placing a magnet on one side of the container to adsorb the super hydrophobic cobalt ferrite; Step e: Tilt the container to drain the liquid in the container.

[0012] In a preferred technical solution of the present invention, after step e, the method further includes: The capture capacity of the powder is calculated according to formula (1): (1); Wherein, m0 is the mass of microplastics dropped into water, m1 is the mass of microplastics captured by the superhydrophobic cobalt ferrite in the container, and Capture Capacity is the capture capacity of the powder; (2); Among them, c1 is the concentration of microplastics dropped into water, and c2 is the concentration of microplastics captured by the superhydrophobic cobalt ferrite in the beaker.

[0013] The third object of the present invention is to provide an application of super hydrophobic cobalt ferrite in water-oil separation, including: (f) Place a 20 μL color development droplet into the water-oil mixture; (g) adding the super hydrophobic cobalt ferrite into the water-oil mixture, and letting the super hydrophobic cobalt ferrite and the water-oil mixture stand for 10 minutes; (h) recovering the superhydrophobic cobalt ferrite using a magnet.

[0014] In a preferred technical solution of the present invention, the water-oil mixture includes any one of hexane, petroleum ether, xylene and olive oil.

[0015] The beneficial effects of the present invention are: The present invention provides a method for preparing a super-hydrophobic cobalt ferrite, comprising step 1: mixing a FeCl3.6H2O solution and a CoCl2.6H2O solution to obtain a mixed solution. Step 2: adding octanoic acid and NaOH solution to the mixed solution in sequence. Step 3: stirring, cooling, rinsing, drying and heat treating the solution in step 2 to obtain cobalt ferrite. Step 4: dissolving lauric acid in anhydrous ethanol to obtain a modified solution. Step 5: adding cobalt ferrite to the modified solution, placing it at room temperature for a first time, and using a magnet to absorb the modified solution; rinsing and drying the cobalt ferrite after the reaction to obtain a super-hydrophobic cobalt ferrite. The above-mentioned preparation method is based on coprecipitation and surface modification, lauric acid is adsorbed on the surface of cobalt ferrite, and the cobalt ferrite is surface-modified to produce a super-hydrophobic cobalt ferrite with stable hydrophobicity and magnetism. Since cobalt ferrite is magnetic, it can be recycled and reused using a permanent magnet. After adding superhydrophobic cobalt ferrite, microplastics and superhydrophobic cobalt ferrite form floccules. At different microplastic concentrations, superhydrophobic cobalt ferrite can efficiently adsorb microplastics, and the removal efficiency of microplastics is close to 100%. The surface functionalized superhydrophobic cobalt ferrite has superoleophilic and superhydrophobic properties. In a water-oil mixture, superhydrophobic cobalt ferrite can wrap oil droplets and form spheres underwater, thereby achieving water-oil separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a schematic diagram of the SEM of superhydrophobic cobalt ferrite; Figure 2 is a schematic diagram of XRD of superhydrophobic cobalt ferrite; Figure 3 is a schematic diagram of the hysteresis loop of superhydrophobic cobalt ferrite; Figure 4(a) is the surface static water contact angle WCA of cobalt ferrite before modification; (b) is the surface static oil contact angle OCA of modified cobalt ferrite; (c) is the surface static water contact angle WCA of cobalt ferrite after modification; (d) is the surface static oil contact angle OCA of cobalt ferrite after modification; Figure 5 It is a schematic diagram of the scene of the surface contact angle under solutions with different pH values; Figure 6 It is the statistical result diagram of the surface contact angle under different pH value solutions; Figure 7 is a schematic diagram of the separation efficiency of superhydrophobic cobalt ferrite in the oil-water separation cycle; Figure 8 is a schematic diagram of the microplastic removal efficiency of superhydrophobic cobalt ferrite; Fig. 9 is a graph of the measurement results of the surface contact angle during the microplastic removal cycle. DETAILED DESCRIPTION

[0017] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0018] Example 1 This embodiment provides a method for preparing a super-hydrophobic cobalt ferrite, comprising the following steps: Step 1: Mixing FeCl3.6H2O solution and CoCl2.6H2O solution to obtain a mixed solution; Step 2: adding octanoic acid and NaOH solution to the mixed solution in sequence; Step 3: stirring, cooling, rinsing, drying and heat treating the solution in step 2 to obtain cobalt ferrite; Step 4: dissolving lauric acid in anhydrous ethanol to obtain a modified solution; Step 5: adding the cobalt ferrite to the modified solution, leaving it at room temperature for a first period of time, and using a magnet to absorb the modified solution; rinsing and drying the cobalt ferrite after the reaction to obtain superhydrophobic cobalt ferrite.

[0019] Prepare two 25 ml portions of FeCl3.6H2O solution (Scharlau, AR) and CoCl2.6H2O solution (Scharlau, AR) in deionized water until the salt is completely dissolved. The ratio of the concentration of FeCl3.6H2O solution to the concentration of CoCl2.6H2O solution is 2:1, the concentration range of FeCl3.6H2O solution is 0.01-0.4mol / L, and the concentration range of CoCl2.6H2O solution is 0.005-0.2mol / L. This example takes the concentration of FeCl3.6H2O solution as 0.4mol / L and the concentration of CoCl2.6H2O solution as 0.2mol / L as an example. After dissolution, mix and add 0.1-2 ml of octanoic acid (Scharlau, AR) dropwise under vigorous and continuous stirring. Next, slowly add a 1.5mol / L NaOH (Scharlau, AR) solution until the desired pH value (7.5≤pH≤8.5) is reached. The resulting solution was stirred at 80°C for 1 hour, and then the resulting product was cooled to room temperature. The main byproduct of the reaction was washed three times with deionized water and then centrifuged at 1500 rpm for 2 minutes. The solid obtained after washing was placed in an oven at 80°C for 8 hours and finally heat-treated at 900°C for 1 hour to obtain cobalt ferrite.

[0020] Weigh 0.5 g of lauric acid (C 12 H 24 O2, Scharlau, AR) is dissolved in 5 ml of anhydrous ethanol, cobalt ferrite is added to the solution, and placed at room temperature for 24 hours. It is preferred to place a magnet under the container to increase the surface area. After 24 hours, the lauric acid solution is sucked away by a magnet, and the surface-modified cobalt ferrite is rinsed with anhydrous ethanol. Finally, the surface-modified cobalt ferrite is placed in the air to dry to obtain superhydrophobic cobalt ferrite. Lauric acid produced by Scharlau is used. AR is the abbreviation of Analytical Reagent, which is analytically pure. Analytical purity is a purity specification of chemical reagents.

[0021] like Figure 1 As shown, a JEOL J-7100 field emission scanning electron microscope (FE-SEM) coupled with an energy dispersive spectroscopy (EDS) detector was used to evaluate the morphology, semi-quantitative composition and particle distribution of the powders, and to investigate the sample surface.

[0022] like Figure 2 As shown, the phase structure of the surface modified cobalt ferrite was examined using X-ray diffraction (PANalytical X'Pert PRO MPD, radiation Fe filtered Co K, wavelength of 1.79 Å).

[0023] like Figure 3As shown, changes in magnetic parameters were measured at 300K using Quantum Design's MPMS XL superconducting quantum interference device (SQUID) magnetometer.

[0024] like Figure 4 Surface contact angles shown: Static water contact angle (WCA) and sliding angle (SA) images were taken at room temperature using a Levenhuk digital microscope using a fixed method with 3 μL of deionized water. Static oil contact angle (OCA) was measured using Hexane, and all contact angles were measured using ImageJ software.

[0025] like Figure 5-Figure 6 As shown, solutions of different pH values ​​(1, 3, 5, 7, 9, 11 and 13) were prepared with HCl and NaOH (Scharlau, AR). The powder was then spread on a glass slide with double-sided tape and pressed with glass to ensure that the powder was evenly distributed on the glass slide. The surface contact angle (CA) and sliding angle (SA) of the powder were then tested using solutions of different pH values. The test was performed 3 to 5 times in solutions of different pH values ​​to ensure the reliability and stability of the data.

[0026] The preparation method of the super-hydrophobic cobalt ferrite provided in the present embodiment comprises step 1: mixing a FeCl3.6H2O solution and a CoCl2.6H2O solution to obtain a mixed solution. Step 2: adding octanoic acid and NaOH solution sequentially to the mixed solution. Step 3: stirring, cooling, rinsing, drying and heat treating the solution in step 2 to obtain cobalt ferrite. Step 4: dissolving lauric acid in anhydrous ethanol to obtain a modified solution. Step 5: adding cobalt ferrite to the modified solution, placing it at room temperature for the first time, and using a magnet to absorb the modified solution; rinsing and drying the cobalt ferrite after the reaction to obtain a super-hydrophobic cobalt ferrite. The above-mentioned preparation method is based on coprecipitation and surface modification, lauric acid is adsorbed on the surface of cobalt ferrite, and the cobalt ferrite is surface-modified to produce a super-hydrophobic cobalt ferrite with stable hydrophobicity and magnetism. Since cobalt ferrite is magnetic, it can be recycled and reused using a permanent magnet. After adding superhydrophobic cobalt ferrite, microplastics and superhydrophobic cobalt ferrite form floccules. At different microplastic concentrations, superhydrophobic cobalt ferrite can efficiently adsorb microplastics, and the removal efficiency of microplastics is close to 100%. The surface functionalized superhydrophobic cobalt ferrite has superoleophilic and superhydrophobic properties. In a water-oil mixture, superhydrophobic cobalt ferrite can wrap oil droplets and form spheres underwater, thereby achieving water-oil separation.

[0027] Example 2 This embodiment provides the application of the super-hydrophobic cobalt ferrite in Example 1 in removing microplastics, including: Step a: Take 5 ml of water and place it in a container, then add different amounts of microplastics; Step b: stirring the water and microplastics in the container; Step c: placing the super hydrophobic cobalt ferrite into the container; Step d: placing a magnet on one side of the container to adsorb the super hydrophobic cobalt ferrite; Step e: Tilt the container to drain the liquid in the container.

[0028] After step e, the method further comprises: The capture capacity of the powder is calculated according to formula (1): (1); Wherein, m0 is the mass of microplastics dropped into water, m1 is the mass of microplastics captured by the superhydrophobic cobalt ferrite in the container, and Capture Capacity is the capture capacity of the powder; The removal efficiency of microplastics is calculated according to formula (2): (2); Among them, c1 is the concentration of microplastics dropped into water, and c2 is the concentration of microplastics captured by the superhydrophobic cobalt ferrite in the beaker.

[0029] High-density polyethylene (HDPE) with a particle size of 99-167 μm was used to test the capture capacity of cobalt ferrite. 5 ml of water was placed in a glass bottle, and different amounts of microplastics were added. The mixture was stirred and ultrasonically dispersed for a certain period of time. Since microplastics have superhydrophobic properties, they all float on the water surface. Then a small amount of powder was added, and under the action of a magnet, the powder was guided to capture the microplastics. Finally, a magnet was placed on one side of the glass bottle to adsorb the magnetic powder, and then the glass bottle was tilted to drain the liquid. The capture capacity of the powder was calculated according to formula (1), and the removal efficiency of microplastics was calculated by formula (2). The results are shown in the figure. Figure 8-Figure 9 shown.

[0030] Example 3 This embodiment provides the application of the super-hydrophobic cobalt ferrite in Example 1 in water-oil separation, including: (f) Place a 20 μL color development droplet into the water-oil mixture; (g) adding the super hydrophobic cobalt ferrite into the water-oil mixture, and letting the super hydrophobic cobalt ferrite and the water-oil mixture stand for 10 minutes; (h) recovering the superhydrophobic cobalt ferrite using a magnet.

[0031] The water-oil mixture includes any one of hexane, petroleum ether, xylene and olive oil.

[0032] The surface contact angle test shows that the surface functionalized cobalt ferrite has selective wettability (superoleophilic and superhydrophobic). In order to explore the application potential and separation efficiency of the prepared superhydrophobic cobalt ferrite in oil-water separation, four different organic solvents (as oil) were used for oil-water separation experiments, namely hexane, petroleum ether, xylene and olive oil. First, 20 μL of oil red color droplets were placed in water, and then a small amount (10-32 mg) of cobalt ferrite powder was added. The particles and the water-oil mixture were left to stand for 10 minutes. It was observed that the area of ​​oil on the water surface gradually decreased and gathered into the cobalt ferrite powder until the red color on the water surface completely disappeared. After capturing a large number of oil droplets, the superhydrophobic cobalt ferrite was observed to form spheres underwater, called oil marbles, which settled to the bottom of the glass bottle. The oil marbles were produced by cobalt ferrite encapsulating oil particles. Finally, the superhydrophobic cobalt ferrite was recovered using a magnet and the mass of the superhydrophobic cobalt ferrite was weighed.

[0033] (3); Wherein, V0 is the volume of oil in the oil-water mixture, V1 is the volume of oil lost after the oil is separated by superhydrophobic cobalt ferrite, and η is the separation efficiency.

[0034] (4); Wherein, m0 is the mass of superhydrophobic cobalt ferrite before oil-water separation, m1 is the mass of superhydrophobic cobalt ferrite after oil-water separation, and Q is the adsorption capacity.

[0035] According to formula (3)-formula (4), the separation efficiency and adsorption capacity of superhydrophobic cobalt ferrite powder for oil-water separation of oil-water mixture can be calculated. In terms of separation efficiency, the separation efficiency of superhydrophobic cobalt ferrite powder in four water-oil mixtures is higher than 94.2%. Among them, the separation of hexane and water mixture is even better, with a separation efficiency of 99.6%. In terms of adsorption capacity, superhydrophobic cobalt ferrite powder has an excellent adsorption capacity for olive oil, which is 1.45 g / g. Furthermore, taking hexane as an example, we studied the separation efficiency of hexane in removing microplastics 10 times. The experimental results are as follows Figure 7 The efficiency of the 10 test results was stable and maintained above 93%. From the separation results, it can be judged that the powder has the ability to separate oil-water mixtures, in which the oil is light oil or heavy oil.

[0036] Table 1 Separation effect of superhydrophobic cobalt ferrite on different water-oil mixtures Ethane Petroleum ether Xylene olive oil η (%) 99.6% 99.2% 96.0% 94.2% Q (g / g) 0.59 0.47 0.81 1.45 Example 4 The present embodiment provides the application of the super-hydrophobic cobalt ferrite in microplastic removal in Example 1, and uses super-hydrophobic cobalt ferrite to carry out microplastic removal experiment under different microplastic concentrations by means of permanent magnet.After removing microplastics each time, it is cleaned with ethanol, and placed in a fume hood for drying and then recycled.The removal efficiency of microplastics in each experiment is calculated, and the surface contact angle of the super-hydrophobic cobalt ferrite after test recovery is tested.After adding super-hydrophobic cobalt ferrite, microplastics and super-hydrophobic cobalt ferrite form floccules.Then, under the attraction of permanent magnet, super-hydrophobic cobalt ferrite and microplastics approach permanent magnet together.The surface functionalization of lauric acid makes the surface of super-hydrophobic cobalt ferrite have stable super-hydrophobic characteristics, and the super-hydrophobic cobalt ferrite modified by lauric acid surface functionalization is subjected to spatial interference caused by the long chain structure attached to the surface of super-hydrophobic cobalt ferrite when contacting the water surface.

[0037] The removal capacity of superhydrophobic cobalt ferrite at different microplastic concentrations was tested. Using 0.01 g of superhydrophobic cobalt ferrite, it was able to efficiently adsorb microplastics at a concentration of 0.1-0.9 mmol / ml. The adsorption capacity of superhydrophobic cobalt ferrite for microplastics was calculated according to formula (2), and the calculation results are shown in Table 2.

[0038] (2); Among them, c1 is the concentration of microplastics dropped into water, and c2 is the concentration of microplastics captured by the superhydrophobic cobalt ferrite in the beaker.

[0039] At different microplastic concentrations, the removal efficiency is close to 100%, and the ability of superhydrophobic cobalt ferrite particles to capture microplastics increases with the increase of microplastic concentration. When there is 0.9 mmol / ml of microplastics in the aqueous solution, 0.01g of superhydrophobic cobalt ferrite is added, and the microplastic capture capacity is 2.56g / g.

[0040] After each removal of microplastics, the superhydrophobic cobalt ferrite was recycled. The contact angle of the superhydrophobic cobalt ferrite particles was measured after each cycle. Figure 8 As shown in Figure 2, the average microplastic removal efficiency in 10 microplastic recycling experiments was as high as 98%. Fig. 9As shown, even after 10 cycles of microplastic removal, the surface contact angle of the superhydrophobic cobalt ferrite is still greater than 150°, showing stable and excellent superhydrophobic performance. After the first 5 cycles of microplastic removal, the surface rolling angle of the superhydrophobic cobalt ferrite did not change much and was close to 0°. It was not until the 6th microplastic removal that the rolling angle of the superhydrophobic cobalt ferrite increased to about 2.6°. After 10 cycles of microplastic removal, the surface rolling angle of the superhydrophobic cobalt ferrite increased to about 7°. After each recycling, the superhydrophobic cobalt ferrite had a small amount of mass loss, but the loss was small. Due to the stability and superhydrophobicity of the modified particles at different pH values, there was no significant difference in the adsorption capacity of the modified particles in different cycles, and multiple recycling cycles did not affect the performance of the superhydrophobic cobalt ferrite in capturing microplastics. The stability of the superhydrophobic cobalt ferrite may be related to the formation of hydrogen bonds between lauric acid and cobalt ferrite, which is attributed to the unique nanoflower-like layered structure of cobalt ferrite and the spatial interference caused by the long chains of functionalized modified lauric acid. The above microplastic removal experimental results show that superhydrophobic cobalt ferrite has excellent microplastic removal efficiency, tough superhydrophobic properties and recyclability, which makes superhydrophobic cobalt ferrite applicable to a variety of scenarios.

[0041] Table 2 Removal effect of superhydrophobic cobalt ferrite on microplastics of different concentrations Microplastic concentration (mmol / ml) 0.1 0.3 0.5 0.7 0.9 Capture capacity (g / g) 1.31 1.44 1.54 2.36 2.56 Microplastic removal efficiencyξ 99% 99% 99% 99% 99% Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values ​​of the parts and steps set forth in these embodiments do not limit the scope of the application. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a restriction. Therefore, other examples of exemplary embodiments can have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in the subsequent accompanying drawings.

[0042] It should be understood that spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. For example, if the device in the figures is inverted, a device described as "above" or "above" other devices or structures would then be positioned "below" or "below" the other devices or structures. Thus, the exemplary term "above" can include both "above" and "below". The device may also be oriented in other different ways (rotated 90 degrees or at other orientations), and the spatially relative descriptions used herein should be interpreted accordingly.

[0043] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.

[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing super hydrophobic cobalt ferrite, characterized in that, The following steps are involved: Step 1: Mixing FeCl3.6H2O solution and CoCl2.6H2O solution to obtain a mixed solution; Step 2: adding octanoic acid and NaOH solution to the mixed solution in sequence; Step 3: stirring, cooling, rinsing, drying and heat treating the solution in step 2 to obtain cobalt ferrite; Step 4: dissolving lauric acid in anhydrous ethanol to obtain a modified solution; Step 5: adding the cobalt ferrite to the modified solution, leaving it at room temperature for a first period of time, and using a magnet to absorb the modified solution; The cobalt ferrite after the reaction is rinsed and dried to obtain super hydrophobic cobalt ferrite.

2. The preparation method of super hydrophobic cobalt ferrite according to claim 1, wherein The modified solution in step 4 is obtained by dissolving 0.5 g of lauric acid in 5 ml of anhydrous ethanol.

3. The preparation method of super hydrophobic cobalt ferrite according to claim 1, characterized in that, In step 1, the concentration of the FeCl3.6H2O solution is 0.4 mol / L, the concentration of the CoCl2.6H2O solution is 0.2 mol / L, and the volumes of the FeCl3.6H2O solution and the CoCl2.6H2O solution are both 25 ml.

4. The preparation method of super hydrophobic cobalt ferrite according to claim 1, characterized in that, In step 2, the volume of octanoic acid is 0.1-2 ml, and the concentration of the NaOH solution is 1.5 mol / L.

5. The preparation method of super hydrophobic cobalt ferrite according to claim 1, characterized in that, The pH value of the solution in step 2 is 7.5-8.

6. The method for preparing super hydrophobic cobalt ferrite according to claim 1, wherein The stirring time in step 3 is 1 hour, and the stirring temperature is 80°C; the centrifugal time is 2 minutes, and the centrifugal speed is 1500 rpm; the drying temperature is 80°C, and the drying time is 8 hours; the heat treatment time is 1 hour, and the heat treatment temperature is 900°C.

7. The use of the super-hydrophobic cobalt ferrite in microplastic removal according to any one of claims 1 to 6, characterized in that: include: Step a: Take 5 ml of water and place it in a container, then add different amounts of microplastics; Step b: stirring the water and microplastics in the container; Step c: placing the super hydrophobic cobalt ferrite into the container; Step d: placing a magnet on one side of the container to adsorb the super hydrophobic cobalt ferrite; Step e: Tilt the container to drain the liquid in the container.

8. The use of super-hydrophobic cobalt ferrite in microplastic removal according to claim 7, characterized in that, After step e, the method further comprises: The capture capacity of the powder is calculated according to formula (1): (1); Wherein, m0 is the mass of microplastics dropped into water, m1 is the mass of microplastics captured by the superhydrophobic cobalt ferrite in the container, and Capture Capacity is the capture capacity of the powder; The removal efficiency of microplastics is calculated according to formula (2): (2); Among them, c1 is the concentration of microplastics dropped into water, and c2 is the concentration of microplastics captured by the superhydrophobic cobalt ferrite in the beaker.

9. The application of the super hydrophobic cobalt ferrite in water-oil separation based on any one of claims 1 to 6, characterized in that: include: (f) Place a 20 μL color development droplet into the water-oil mixture; (g) adding the super hydrophobic cobalt ferrite into the water-oil mixture, and letting the super hydrophobic cobalt ferrite and the water-oil mixture stand for 10 minutes; (h) recovering the superhydrophobic cobalt ferrite using a magnet.

10. The use of super hydrophobic cobalt ferrite in water-oil separation according to claim 9, characterized in that: The water-oil mixture includes any one of hexane, petroleum ether, xylene and olive oil.

Citation Information

Patent Citations

  • A method for removing microplastics from water medium based on bubble flotation

    CN116143218B

  • Preparation methods of super hydrophobic magnetic powder

    CN101912964A

  • Preparation method of super-hydrophobic magnetic powder

    CN102248158A

Cited By

  • Kitchen biogas residue micro-plastic deep separation method based on in-situ biological membrane stripping and hydrophobic magnetic induction