Normal-temperature ozone decomposition catalyst and preparation method thereof

By pretreatment and activation of honeycomb ceramics, activated carbon and glass fiber filters, and addition of active components, an efficient normal temperature ozone decomposition catalyst is formed, which solves the problem of insufficient catalyst performance in the prior art, and achieves high-efficiency ozone decomposition and The mechanical strength is improved, and the preparation process and cost are optimized.

CN118988278AActive Publication Date: 2024-11-22HANGZHOU ZUNHENG TECHNOLOGY DEVELOPMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411269387.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing ozone decomposition catalysts have insufficient purity, surfactivity, catalytic performance, stability and durability at room temperature, and the preparation process is complex and low efficiency, which fails to effectively improve the ozone decomposition efficiency and mechanical strength.

Method used

By pretreating and activation of honeycomb ceramics and activated carbon, combining with glass fiber filters, adding active components, and using ultrasonic cleaning, pickling, water vapor activation and hot pressing curing technologies, an efficient ozone decomposition catalyst is formed at a temperature of 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% and 100% .

Benefits of technology

It significantly improves the purity, surfactivity and catalytic performance of the catalyst, enhances mechanical strength and durability, optimizes the preparation process, improves the ozone decomposition efficiency and temperature stability, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988278A_ABST
    Figure CN118988278A_ABST
Patent Text Reader

Abstract

The invention discloses a normal-temperature catalyst for ozonolysis and a preparation method thereof, and relates to the technical field of ozonolysis catalysts.The preparation method of the normal-temperature catalyst for ozonolysis comprises the following steps that S1, honeycomb ceramic and activated carbon are pretreated and activated; in the step S1, the method further comprises the following steps: S11, soaking and washing the honeycomb ceramic, and then carrying out ultrasonic cleaning and drying treatment; s12, carrying out high-temperature calcination and acid pickling treatment on the dried honeycomb ceramic; s13, the activated carbon is subjected to screening, soaking and washing, ultrasonic cleaning and acid pickling treatment; and S14, carrying out steam activation treatment on the pretreated activated carbon. The honeycomb ceramic, the activated carbon and the glass fiber-shaped filter screen are pretreated and activated, so that the purity, the surface activity, the catalytic efficiency, the stability and the durability of the catalyst for normal-temperature ozonolysis can be improved, and the preparation process of the catalyst for normal-temperature ozonolysis is optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ozone decomposition catalysts, in particular to a catalyst for normal temperature ozone decomposition and a preparation method thereof. Background Art

[0002] Traditional ozone decomposition catalysts contain impurities, which will reduce the catalytic activity of the catalyst and affect the efficiency of ozone decomposition. The ozone decomposition catalyst of the present application can improve the purity, surface activity, catalytic efficiency, stability and durability of the catalyst for room-temperature ozone decomposition, and optimize the preparation process of the catalyst for room-temperature ozone decomposition.

[0003] The defects of existing ozone decomposition catalysts are:

[0004] 1. Patent document KR101582233B1 discloses an ozone decomposition catalyst, a method for manufacturing the same and a method for decomposing ozone using the same. The document mainly considers the problem of how to obtain satisfactory ozone decomposition efficiency, but does not consider how to improve the purity, surface activity, catalytic efficiency, stability and durability of the catalyst for room-temperature ozone decomposition, and how to optimize the preparation process of the catalyst for room-temperature ozone decomposition;

[0005] 2. Patent document CN114471622B discloses an ozone decomposition catalyst and a preparation method thereof. The document mainly considers the problem of how to obtain an ozone decomposition catalyst with stable properties, high decomposition efficiency and strong moisture resistance, but does not consider how to improve the ozone decomposition efficiency of the catalyst for room-temperature ozone decomposition, enhance the mechanical strength and durability of the catalyst for room-temperature ozone decomposition, and ensure the stability and bonding strength of the structure of the catalyst for room-temperature ozone decomposition;

[0006] 3. Patent document CN110433820B discloses a catalyst for decomposing ozone in gas and a preparation method thereof. The document mainly considers how to solve the problems of complex preparation process, poor binding force between active ingredients and carriers, and serious dust shedding of ozone decomposition catalysts in the prior art, but does not consider how to improve the catalytic activity of the room-temperature ozone decomposition catalyst for ozone decomposition, optimize the catalytic performance of the room-temperature ozone decomposition catalyst, and expand the application range of the room-temperature ozone decomposition catalyst;

[0007] 4. Patent document CN111974380B discloses an ozone decomposition catalyst and a preparation method thereof. The document mainly considers the problem of how to synthesize a new type of high-efficiency ozone decomposition catalyst using a simple process, but does not consider how to optimize the catalyst formula for room-temperature ozone decomposition, evaluate the temperature stability of the catalyst for room-temperature ozone decomposition, and thus reduce the cost of the catalyst for room-temperature ozone decomposition; Summary of the invention

[0008] The object of the present invention is to provide a catalyst for room temperature ozone decomposition and a preparation method thereof to solve the problems raised in the above background technology.

[0009] To achieve the above object, the present invention provides the following technical solutions: a catalyst for room temperature ozone decomposition and a preparation method thereof. The preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0010] Step S1, pretreatment and activation of honeycomb ceramics and activated carbon;

[0011] Step S2, loading the activated carbon onto the honeycomb ceramic carrier;

[0012] Step S3, pretreatment and activation of the glass fiber filter;

[0013] Step S4, compounding the glass fiber filter screen with the honeycomb ceramic carrier loaded with activated carbon;

[0014] Step S5, adding active components;

[0015] Step S6, performing performance testing on the catalyst for normal temperature ozone decomposition;

[0016] In S1, the following steps are also included:

[0017] S11, completely immersing the honeycomb ceramic with a size of 100mm×100mm×100mm in deionized water for 0.5h, rinsing the immersed honeycomb ceramic with deionized water, then putting the rinsed honeycomb ceramic into an ultrasonic cleaning machine, adding deionized water into the ultrasonic cleaning machine, starting the ultrasonic cleaning machine for cleaning for 0.5h, taking the cleaned honeycomb ceramic out of the ultrasonic cleaning machine, and placing the honeycomb ceramic in a drying oven for drying at a drying temperature of 120°C for 2 hours;

[0018] S12, placing the dried honeycomb ceramic in a high temperature furnace, heating the temperature to 400°C at a heating rate of 5°C / min, and keeping the temperature for 3 hours. After the calcination is completed, the high temperature furnace is naturally cooled to room temperature and the honeycomb ceramic is taken out, and the calcined honeycomb ceramic is immersed in a 1 mol / L nitric acid solution for 1 hour, with continuous stirring during the immersion process. After the acid wash is completed, the honeycomb ceramic is thoroughly rinsed with deionized water until the rinse liquid is neutral, and then the rinsed honeycomb ceramic is placed in a drying oven for drying, and the drying temperature and time are the same as those during the pretreatment;

[0019] S13, using a sieve to screen the activated carbon to obtain activated carbon with an average particle size of 10 mm, completely immersing the activated carbon in deionized water for 0.5 h, and rinsing the immersed activated carbon with deionized water, then putting the rinsed activated carbon into an ultrasonic cleaning machine, adding deionized water to the ultrasonic cleaning machine until the water level of the deionized water covers the activated carbon, and starting the ultrasonic cleaning machine for cleaning for 0.5 h;

[0020] The activated carbon was completely immersed in a 1.5 mol / L dilute hydrochloric acid solution for 1 hour. Stirring was continued during the immersion process. After the acid washing was completed, the activated carbon was repeatedly rinsed with deionized water until the rinse liquid was neutral. The rinsed activated carbon was placed in a drying oven for drying at a temperature of 105°C for 2 hours.

[0021] S14. Place the pretreated activated carbon into a steam activation reactor and start heating it to make the activated carbon reach the required activation temperature, which is 700°C. When the activated carbon reaches the activation temperature, introduce steam and keep the activation time for 2 hours. After the activation is completed, stop heating and introducing steam, allow the steam activation reactor to cool naturally to room temperature, and open the steam activation reactor to collect the activated carbon after steam activation.

[0022] Preferably, in S2, the following steps are also included:

[0023] S21, crushing the activated carbon to obtain activated carbon powder with an average particle size of 1 mm, mixing the activated carbon powder with deionized water to form a uniform loading slurry, adding carboxymethyl cellulose as a binder, immersing the pretreated and activated honeycomb ceramic in the loading slurry, and after soaking for 5 hours, taking out the honeycomb ceramic carrier, and using compressed air to remove excess slurry on the surface;

[0024] S22, placing the honeycomb ceramic carrier loaded with activated carbon in a drying oven for drying, the drying temperature is 110° C., and the drying time is 4 hours.

[0025] Preferably, in S3, the following steps are also included:

[0026] S31, putting a glass fiber filter with a size of 100 mm×100 mm×10 mm into a washing machine, adding a neutral detergent, and washing with deionized water for 20 minutes. After washing, rinse the filter with deionized water for multiple times, and put the rinsed glass fiber filter into a drying machine at a drying temperature of 65° C. for 40 minutes;

[0027] S32. Fix the glass fiber filter on the workbench of the sandblasting machine for sandblasting. The sandblasting material is white corundum, the sandblasting pressure is 0.5MPa, the sandblasting distance is 100mm, and the sandblasting time is 1.5h. After the sandblasting is completed, use deionized water to clean and dry the glass fiber filter.

[0028] Preferably, in S4, the following steps are also included:

[0029] S41. A layer of acrylic adhesive is uniformly coated on the surface of the honeycomb ceramic carrier loaded with activated carbon, and the pretreated and activated glass fiber filter is covered on the honeycomb ceramic carrier coated with the acrylic adhesive.

[0030] Preferably, in S4, the following steps are also included:

[0031] S42, placing the honeycomb ceramic carrier composited with the glass fiber filter and loaded with activated carbon in a vacuum chamber, starting the vacuum pump to form a negative pressure environment, the glass fiber filter will be adsorbed onto the honeycomb ceramic carrier to form a preliminary combination with the acrylic adhesive, and a preliminary composite material is obtained;

[0032] S43, taking out the preliminary composite material after vacuum adsorption, placing it in a mechanical pressing device, using a roller press to apply uniform pressure to the preliminary composite material, and then placing the preliminary composite material in a hot press to perform hot pressing curing treatment to obtain a complete composite material.

[0033] Preferably, in S5, the following steps are also included:

[0034] S51. Prepare a precursor solution through the active component precursor, immerse the complete composite material in the precursor solution, fix the active component accounting for 10% of the total mass on the complete composite material, take out the complete composite material, dry it at 120°C for 3h, and calcine it at 500°C for 3h to obtain a catalyst for room temperature ozone decomposition.

[0035] Preferably, the active component precursor is one or more of 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate and nickel nitrate hexahydrate.

[0036] Preferably, in S6, the following steps are also included:

[0037] S61. Precursor solutions are prepared in sequence by 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate, nickel nitrate hexahydrate, 50% manganese nitrate solution and cobalt nitrate hexahydrate, 50% manganese nitrate solution and iron nitrate nonahydrate, 50% manganese nitrate solution and copper nitrate trihydrate, 50% manganese nitrate solution and nickel nitrate hexahydrate, and are numbered 1-9.

[0038] Preferably, in S6, the following steps are also included:

[0039] S62, immersing the complete composite material in the precursor solution 1-9, fixing the active components accounting for 10% of the total mass on the complete composite material, taking out the complete composite material, drying it at 120° C. for 3 h, and calcining it at 500° C. for 3 h, to obtain the room temperature ozone decomposition catalyst 1-9;

[0040] Under the conditions of temperature of 30°C, space velocity of 10000h-1, oxygen concentration of 20vol% and ozone concentration of 100ppmv, the loading amount of the room temperature ozone decomposition catalyst was 2g, and the ozone decomposition efficiency of room temperature ozone decomposition catalysts 1-9 under the same conditions was measured using Eco SensorsUV-100 ozone analyzer to obtain a group of room temperature ozone decomposition catalysts with the highest ozone decomposition efficiency.

[0041] Preferably, in S6, the following steps are also included:

[0042] S63. A group of room-temperature ozone decomposition catalysts with the highest ozone decomposition efficiency were used to measure the ozone decomposition efficiency at temperatures of 30°C, 34°C, 38°C, 42°C, 46°C and 50°C under the conditions of a space velocity of 10,000 h-1, an oxygen concentration of 20 vol% and an ozone concentration of 100 ppmv, using an Eco Sensors UV-100 ozone analyzer.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1. The present invention pre-treats and activates honeycomb ceramics, activated carbon and glass fiber filter screens, and effectively removes impurities and pollutants on the surfaces of honeycomb ceramics, activated carbon and glass fiber filter screens through deionized water immersion, ultrasonic cleaning, high-temperature calcination and acid washing steps, thereby significantly improving the purity of these materials. The high-temperature calcination and acid washing processes can further open the pore structure of honeycomb ceramics and activated carbon, increase the specific surface area, thereby improving the surface activity of the catalyst for room-temperature ozone decomposition, and facilitating the adsorption and decomposition of ozone molecules. The activated carbon is treated with water vapor activation, and its pore structure is further optimized to form more micropores and mesopores. These pore structures provide more adsorption sites and reaction channels for ozone molecules, thereby significantly enhancing the catalytic efficiency of the catalyst for room-temperature ozone decomposition. The glass fiber filter screen is treated with sandblasting. The surface becomes rough, which increases the contact area with ozone molecules, and at the same time removes burrs and uneven parts on the surface, which is beneficial to the uniform distribution and effective decomposition of ozone molecules. Through pretreatment and activation steps, the stability and consistency of the catalyst for room-temperature ozone decomposition during the preparation process are ensured, and performance degradation or failure due to impurities or defects is avoided, thereby improving the preparation efficiency and yield of the catalyst for room-temperature ozone decomposition, and reducing production costs. In addition, the high-temperature calcination process not only removes volatile components in the material, but also enhances the thermal and chemical stability of honeycomb ceramics and activated carbon, enabling them to maintain stable catalytic performance under various environmental conditions. Therefore, it can solve the problems of improving the purity, surface activity, catalytic efficiency, stability and durability of the catalyst for room-temperature ozone decomposition, and optimizing the preparation process of the catalyst for room-temperature ozone decomposition.

[0045] 2. The present invention obtains a completely composite material by loading activated carbon onto a honeycomb ceramic carrier, and compounding a glass fiber filter with the honeycomb ceramic carrier loaded with activated carbon. The activated carbon can effectively adsorb ozone molecules due to its high specific surface area and excellent adsorption performance, thereby promoting the decomposition of ozone. The honeycomb ceramic carrier has good mechanical strength and stability, and can withstand stress changes under various environmental conditions. Loading activated carbon powder onto the honeycomb ceramic carrier can increase the contact area between the activated carbon and ozone, improve the adsorption and decomposition efficiency of ozone, and maintain the catalytic activity of the activated carbon, significantly improving the mechanical strength and durability of the catalyst for room-temperature ozone decomposition. At the same time, the glass fiber filter has good air permeability and filtering performance, can evenly distribute the gas flow, reduce air flow resistance, and enable ozone molecules to more evenly contact the room-temperature The surface of the room-temperature ozone decomposition catalyst can be covered by the glass fiber filter, thereby improving the decomposition efficiency. The glass fiber filter can also block large particles from entering the interior of the room-temperature ozone decomposition catalyst, protecting the room-temperature ozone decomposition catalyst from pollution. By coating an acrylic adhesive on the honeycomb ceramic carrier and using vacuum adsorption and mechanical pressing technology, the glass fiber filter is firmly bonded to the room-temperature ozone decomposition catalyst to form a completely composite material. This bonding method not only enhances the stability of the composite material structure, but also ensures close contact between the filter and the room-temperature ozone decomposition catalyst, thereby improving the mass transfer efficiency of the catalytic reaction. Therefore, it can solve the problems of improving the ozone decomposition efficiency of the room-temperature ozone decomposition catalyst, enhancing the mechanical strength and durability of the room-temperature ozone decomposition catalyst, and ensuring the stability and bonding force of the structure of the room-temperature ozone decomposition catalyst.

[0046] 3. The present invention adds active components to a catalyst for room-temperature ozone decomposition, wherein the active component precursor is one or more of 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate and nickel nitrate hexahydrate, and configures a precursor solution through the active component precursor, immerses the complete composite material in the precursor solution, and after the active components accounting for 10% of the total mass are fixed on the complete composite material, the complete composite material is taken out, and dried at 120°C for 3h, and calcined at 500°C for 3h to obtain a catalyst for room-temperature ozone decomposition. The active components serve as active sites in the catalyst for room-temperature ozone decomposition to promote the adsorption and decomposition of ozone molecules. By introducing these active components into the catalyst, the The ability of the room-temperature ozone decomposition catalyst to decompose ozone. Calcination of the room-temperature ozone decomposition catalyst at high temperature can make its structure more stable and reduce the performance degradation caused by structural changes during use. At the same time, the interaction between the active components and the carrier will also be strengthened, thereby improving the durability and stability of the room-temperature ozone decomposition catalyst. The active components are fixed on a completely composite material by an impregnation method. This method is simple to operate and easy to control, and can ensure the uniform distribution of the active components in the catalyst. Therefore, it can solve the problem of improving the catalytic activity of the room-temperature ozone decomposition catalyst for ozone decomposition, optimizing the catalytic performance of the room-temperature ozone decomposition catalyst, and expanding the application range of the room-temperature ozone decomposition catalyst.

[0047] 4. The present invention measures the ozone decomposition efficiency of room-temperature ozone decomposition catalysts with different active components added under the same conditions, and measures the ozone decomposition efficiency of a group of room-temperature ozone decomposition catalysts with the highest ozone decomposition efficiency at temperatures of 30°C, 34°C, 38°C, 42°C, 46°C and 50°C. By comparing the ozone decomposition efficiencies of room-temperature ozone decomposition catalysts prepared with different active components and combinations of active components, it is possible to determine which or which combinations of active components have the highest catalytic activity under specific conditions, which is helpful to optimize the formula of room-temperature ozone decomposition catalysts and improve the efficiency of ozone decomposition. After determining the ozone decomposition efficiency with the highest After the room-temperature ozone decomposition catalyst is combined, the ozone decomposition efficiency of the room-temperature ozone decomposition catalyst at different temperatures is further measured, the temperature stability of the room-temperature ozone decomposition catalyst can be evaluated, and the optimal operating temperature range of the room-temperature ozone decomposition catalyst performance can be identified, which is helpful to achieve the best ozone decomposition effect. In practical applications, ozone can be more effectively decomposed, energy consumption and operating costs can be reduced, and the overall economy and practicality can be improved. Therefore, the problem of optimizing the formula of the room-temperature ozone decomposition catalyst, evaluating the temperature stability of the room-temperature ozone decomposition catalyst, and thus reducing the cost of the room-temperature ozone decomposition catalyst can be solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 It is a preparation flow chart of the present invention. DETAILED DESCRIPTION

[0049] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] Embodiment 1,

[0051] See also Figure 1 , an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0052] Step S1, pretreatment and activation of honeycomb ceramics and activated carbon;

[0053] In S1, the following steps are also included:

[0054] S11, completely immersing the honeycomb ceramic with a size of 100mm×100mm×100mm in deionized water for 0.5h, rinsing the immersed honeycomb ceramic with deionized water, then putting the rinsed honeycomb ceramic into an ultrasonic cleaning machine, adding deionized water into the ultrasonic cleaning machine, starting the ultrasonic cleaning machine for cleaning for 0.5h, taking the cleaned honeycomb ceramic out of the ultrasonic cleaning machine, and placing the honeycomb ceramic in a drying oven for drying at a drying temperature of 120°C for 2 hours;

[0055] S12, placing the dried honeycomb ceramic in a high temperature furnace, heating the temperature to 400°C at a heating rate of 5°C / min, and keeping the temperature for 3 hours. After the calcination is completed, the high temperature furnace is naturally cooled to room temperature and the honeycomb ceramic is taken out, and the calcined honeycomb ceramic is immersed in a 1 mol / L nitric acid solution for 1 hour, with continuous stirring during the immersion process. After the acid wash is completed, the honeycomb ceramic is thoroughly rinsed with deionized water until the rinse liquid is neutral, and then the rinsed honeycomb ceramic is placed in a drying oven for drying, and the drying temperature and time are the same as those during the pretreatment;

[0056] S13, using a sieve to screen the activated carbon to obtain activated carbon with an average particle size of 10 mm, completely immersing the activated carbon in deionized water for 0.5 h, and rinsing the immersed activated carbon with deionized water, then putting the rinsed activated carbon into an ultrasonic cleaning machine, adding deionized water to the ultrasonic cleaning machine until the water level of the deionized water covers the activated carbon, and starting the ultrasonic cleaning machine for cleaning for 0.5 h;

[0057] The activated carbon was completely immersed in a 1.5 mol / L dilute hydrochloric acid solution for 1 hour. Stirring was continued during the immersion process. After the acid washing was completed, the activated carbon was repeatedly rinsed with deionized water until the rinse liquid was neutral. The rinsed activated carbon was placed in a drying oven for drying at a temperature of 105°C for 2 hours.

[0058] S14. Place the pretreated activated carbon into a steam activation reactor and start heating it to make the activated carbon reach the required activation temperature, which is 700°C. When the activated carbon reaches the activation temperature, introduce steam and keep the activation time for 2 hours. After the activation is completed, stop heating and introducing steam, allow the steam activation reactor to cool naturally to room temperature, and open the steam activation reactor to collect the activated carbon after steam activation.

[0059] Furthermore, using deionized water to soak and ultrasonically clean the honeycomb ceramics can remove surface impurities and dirt in the pores. Drying treatment ensures that the performance of the honeycomb ceramics will not be affected by moisture in subsequent steps. High-temperature calcination can remove volatile substances in the honeycomb ceramics and enhance their structural stability. Soaking and stirring in nitric acid solution helps to further purify the surface of the honeycomb ceramics, remove residual impurities, and increase the surface roughness through acid washing, which is beneficial to the subsequent loading of the catalyst.

[0060] Activated carbon with uniform particle size is obtained through sieve screening to ensure its uniform distribution in the catalyst. Dust and impurities on the surface of the activated carbon are removed by deionized water immersion and ultrasonic cleaning. The surface of the activated carbon is further purified by immersion in dilute hydrochloric acid solution to remove possible metal ions and other impurities. Steam activation is a key step in improving the adsorption performance of activated carbon. Through high-temperature steam treatment, the pore structure of the activated carbon can be opened, its specific surface area and adsorption capacity can be increased. The activated carbon will have better catalytic activity, which is beneficial to the decomposition of ozone.

[0061] Embodiment 2:

[0062] See also Figure 1 , an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0063] Step S2, loading the activated carbon onto the honeycomb ceramic carrier;

[0064] In S2, the following steps are also included:

[0065] S21, crushing the activated carbon to obtain activated carbon powder with an average particle size of 1 mm, mixing the activated carbon powder with deionized water to form a uniform loading slurry, adding carboxymethyl cellulose as a binder, immersing the pretreated and activated honeycomb ceramic in the loading slurry, and after soaking for 5 hours, taking out the honeycomb ceramic carrier, and using compressed air to remove excess slurry on the surface;

[0066] S22, placing the honeycomb ceramic carrier loaded with activated carbon in a drying oven for drying, the drying temperature is 110° C., and the drying time is 4 hours.

[0067] Furthermore, the activated carbon was crushed into powder with an average particle size of 1 mm, ensuring that the activated carbon could be evenly distributed in the pores and surface of the honeycomb ceramic, thereby improving the catalytic efficiency. The activated carbon powder was mixed with an appropriate amount of deionized water to form a uniform loading slurry. Carboxymethyl cellulose was added to the loading slurry as a binder, which could effectively adhere the activated carbon powder to the honeycomb ceramic carrier. By adjusting the amount of carboxymethyl cellulose added, the viscosity of the loading slurry and the loading amount of the activated carbon could be controlled.

[0068] The pretreated and activated honeycomb ceramics were completely immersed in the loading slurry for 5 hours to ensure that the activated carbon could fully penetrate into the pores of the honeycomb ceramics and adhere to its surface. After the immersion was completed, the excess slurry on the surface of the honeycomb ceramic carrier was removed by compressed air to avoid the catalyst layer being too thick and affecting its permeability and catalytic efficiency.

[0069] The honeycomb ceramic carrier loaded with activated carbon is placed in a drying oven for drying. The drying temperature is set to 110°C and the drying time is 4 hours to ensure that the water is fully evaporated without affecting the structure and performance of the honeycomb ceramic carrier. After drying, the activated carbon powder loaded on the honeycomb ceramic carrier will form a uniform catalytic layer. This catalytic layer not only has a large specific surface area and rich pore structure, but also forms a strong bond with the honeycomb ceramic carrier, thereby ensuring the stability and durability of the catalyst.

[0070] Embodiment 3,

[0071] See also Figure 1 , an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0072] Step S3, pretreatment and activation of the glass fiber filter;

[0073] In S3, the following steps are also included:

[0074] S31, putting a glass fiber filter with a size of 100 mm×100 mm×10 mm into a washing machine, adding a neutral detergent, and washing with deionized water for 20 minutes. After washing, rinse the filter with deionized water for multiple times, and put the rinsed glass fiber filter into a drying machine at a drying temperature of 65° C. for 40 minutes;

[0075] S32. Fix the glass fiber filter on the workbench of the sandblasting machine for sandblasting. The sandblasting material is white corundum, the sandblasting pressure is 0.5MPa, the sandblasting distance is 100mm, and the sandblasting time is 1.5h. After the sandblasting is completed, use deionized water to clean and dry the glass fiber filter.

[0076] Furthermore, a glass fiber filter with a size of 100 mm × 100 mm × 10 mm was placed in a washing machine, and an appropriate amount of neutral detergent was added. The neutral detergent was selected to avoid damage to the filter material and effectively remove oil and dust on the filter surface. Deionized water was used for washing for 20 minutes to ensure that the detergent was fully dissolved and impurities were removed.

[0077] After washing, the filter is rinsed with deionized water for several times to completely remove the residual detergent and impurities. Then, the rinsed glass fiber filter is placed in a dryer at a drying temperature of 65°C for 40 minutes. The purpose of this step is to remove moisture from the surface of the filter to prevent it from becoming moldy or affecting the loading effect of the catalyst during subsequent processing.

[0078] The purpose of sandblasting is to improve the surface roughness of the glass fiber filter, increase its contact area and adhesion with the active components of the catalyst, and remove the unfavorable factors such as the oxide layer and rust spots on the surface of the glass fiber filter through sandblasting, so that the surface of the glass fiber filter is smoother and more uniform. The washed and dried glass fiber filter is fixed on the workbench of the sandblasting machine, and white corundum is selected as the sandblasting material. White corundum has moderate hardness and will not cause excessive damage to the glass fiber filter. At the same time, it can effectively remove surface impurities. The sandblasting pressure is set to 0.5MPa, the sandblasting distance is 100mm, and the sandblasting time is 1.5 hours to ensure the best sandblasting effect.

[0079] After the sandblasting is completed, the glass fiber filter is cleaned with deionized water to remove dust and impurities generated during the sandblasting process. Subsequently, the glass fiber filter is placed in a drying oven for drying to ensure that there is no moisture residue on the surface of the glass fiber filter.

[0080] Embodiment 4:

[0081] See also Figure 1, an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0082] Step S4, compounding the glass fiber filter screen with the honeycomb ceramic carrier loaded with activated carbon;

[0083] In S4, the following steps are also included:

[0084] S41. A layer of acrylic adhesive is uniformly coated on the surface of the honeycomb ceramic carrier loaded with activated carbon, and the pretreated and activated glass fiber filter is covered on the honeycomb ceramic carrier coated with the acrylic adhesive.

[0085] S42, placing the honeycomb ceramic carrier composited with the glass fiber filter and loaded with activated carbon in a vacuum chamber, starting the vacuum pump to form a negative pressure environment, the glass fiber filter will be adsorbed onto the honeycomb ceramic carrier to form a preliminary combination with the acrylic adhesive, and a preliminary composite material is obtained;

[0086] S43, taking out the preliminary composite material after vacuum adsorption, placing it in a mechanical pressing device, using a roller press to apply uniform pressure to the preliminary composite material, and then placing the preliminary composite material in a hot press to perform hot pressing curing treatment to obtain a complete composite material.

[0087] Further, first, a layer of acrylic adhesive is evenly coated on the surface of the honeycomb ceramic carrier loaded with activated carbon, the acrylic adhesive has good bonding performance and weather resistance, and can ensure the firm bonding between the glass fiber filter and the honeycomb ceramic carrier, and then, the pre-treated and activated glass fiber filter is covered on the honeycomb ceramic carrier coated with the acrylic adhesive, ensuring the alignment and close contact between the filter and the carrier, so that the adhesive can fully play its role;

[0088] The honeycomb ceramic carrier composited with the glass fiber filter and loaded with activated carbon is placed in a vacuum chamber, and a vacuum pump is started to form a negative pressure environment. Under the action of negative pressure, the glass fiber filter will be adsorbed onto the honeycomb ceramic carrier and initially bonded with the acrylic adhesive. This step helps to remove air and impurities between the filter and the carrier and improve the bonding strength. After vacuum adsorption, a preliminary composite material is obtained. At this time, a relatively stable bond has been formed between the glass fiber filter and the honeycomb ceramic carrier, but further curing treatment is required to enhance its durability.

[0089] The preliminary composite material after vacuum adsorption is taken out and placed in a mechanical pressing device, and a roller press is used to apply uniform pressure to the preliminary composite material to further compact the bonding layer between the glass fiber filter and the honeycomb ceramic carrier and eliminate possible tiny gaps;

[0090] Next, the preliminary composite material is placed in a hot press for hot pressing and curing treatment. The hot pressing and curing treatment can cause the acrylic adhesive to undergo a chemical reaction at high temperature to form a stronger chemical bond, thereby enhancing the bonding strength between the glass fiber filter and the honeycomb ceramic carrier. At the same time, the hot pressing treatment also helps to improve the overall stability and durability of the composite glass fiber filter and the honeycomb ceramic carrier. After the hot pressing and curing treatment, a completely composite material is obtained.

[0091] Embodiment 5,

[0092] See also Figure 1 , an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0093] Step S5, adding active components;

[0094] In S5, the following steps are also included:

[0095] S51. Prepare a precursor solution through the active component precursor, immerse the complete composite material in the precursor solution, fix the active component accounting for 10% of the total mass on the complete composite material, take out the complete composite material, dry it at 120°C for 3h, and calcine it at 500°C for 3h to obtain a catalyst for room temperature ozone decomposition.

[0096] The active component precursor is one or more of 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate and nickel nitrate hexahydrate.

[0097] Further, the fully composite material after the composite treatment is immersed in the precursor solution 1-9 respectively, and the immersion time should be long enough to ensure that the precursor solution 1-9 can fully penetrate into the pores and surface of the fully composite material, so as to fix the active components accounting for 10% of the total mass. After the immersion is completed, the fully composite material is gently taken out to avoid excessive dripping of the precursor solution 1-9;

[0098] The complete composite material impregnated with the precursor solution is placed in a drying oven and dried at 120° C. for 3 hours to ensure that the solvent in the precursor solution is completely evaporated and the precursor forms a uniform coating on the surface of the complete composite material;

[0099] After drying, the fully composite material is placed in a high-temperature furnace and calcined at 500°C for 3 hours. The purpose of this step is to cause the precursor to undergo thermal decomposition reaction and convert it into catalytically active oxides or composite oxides, and to further improve the crystallinity and stability of the catalyst for room-temperature ozone decomposition. At the same time, calcination also helps to remove organic impurities and volatile substances that may remain in the catalyst for room-temperature ozone decomposition.

[0100] Embodiment 6,

[0101] See also Figure 1 , an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0102] Step S6, testing the ozone decomposition performance of the catalyst for room temperature ozone decomposition;

[0103] In S6, the following steps are also included:

[0104] S61. Precursor solutions are prepared in sequence by 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate, nickel nitrate hexahydrate, 50% manganese nitrate solution and cobalt nitrate hexahydrate, 50% manganese nitrate solution and iron nitrate nonahydrate, 50% manganese nitrate solution and copper nitrate trihydrate, 50% manganese nitrate solution and nickel nitrate hexahydrate, and are numbered 1-9.

[0105] S62, immersing the complete composite material in the precursor solution 1-9, fixing the active components accounting for 10% of the total mass on the complete composite material, taking out the complete composite material, drying it at 120° C. for 3 h, and calcining it at 500° C. for 3 h, to obtain the room temperature ozone decomposition catalyst 1-9;

[0106] Under the conditions of temperature of 30°C, space velocity of 10000h-1, oxygen concentration of 20vol% and ozone concentration of 100ppmv, the loading amount of the room temperature ozone decomposition catalyst was 2g, and the ozone decomposition efficiency of room temperature ozone decomposition catalysts 1-9 under the same conditions was measured using Eco SensorsUV-100 ozone analyzer to obtain a group of room temperature ozone decomposition catalysts with the highest ozone decomposition efficiency.

[0107] Furthermore, the measurement results are as follows:

[0108] serial number Active ingredient precursor Ozone decomposition efficiency (%) 1 50% manganese nitrate solution 52.4 2 Cobalt nitrate hexahydrate 34.8 3 Iron nitrate nonahydrate 36.8 4 Copper nitrate trihydrate 27.5 5 Nickel nitrate hexahydrate 37.2 6 50% manganese nitrate solution and cobalt nitrate hexahydrate 69.4 7 50% manganese nitrate solution and ferric nitrate nonahydrate 96.1 8 50% manganese nitrate solution and copper nitrate trihydrate 92.6 9 50% manganese nitrate solution and nickel nitrate hexahydrate 74.8

[0109] The measurement results show that the catalyst 7 for room temperature ozone decomposition was prepared using a precursor solution 7 prepared from 50% manganese nitrate solution and iron nitrate nonahydrate. The ozone decomposition efficiency was maximum under the conditions of a temperature of 30°C, a space velocity of 10000h-1, an oxygen concentration of 20vol%, an ozone concentration of 100ppmv and a loading amount of 2g of the catalyst for room temperature ozone decomposition.

[0110] Embodiment 7,

[0111] See also Figure 1, an embodiment provided by the present invention: a catalyst for room temperature ozone decomposition and a preparation method thereof, the preparation method of the catalyst for room temperature ozone decomposition is as follows:

[0112] Step S6, testing the ozone decomposition performance of the catalyst for room temperature ozone decomposition;

[0113] In S6, the following steps are also included:

[0114] S63. A group of room-temperature ozone decomposition catalysts with the highest ozone decomposition efficiency were used to measure the ozone decomposition efficiency at temperatures of 30°C, 34°C, 38°C, 42°C, 46°C and 50°C under the conditions of a space velocity of 10,000 h-1, an oxygen concentration of 20 vol% and an ozone concentration of 100 ppmv, using an Eco Sensors UV-100 ozone analyzer.

[0115] Further, a group of room-temperature ozone decomposition catalysts with the highest ozone decomposition efficiency is room-temperature ozone decomposition catalyst 7;

[0116] The measurement results are as follows:

[0117] Temperature(℃) 30 34 38 42 46 50 Ozone decomposition efficiency (%) 96.1 98.2 99.6 99.7 99.8 99.6

[0118] The measurement results show that when the temperature is 30℃-46℃, the ozone decomposition efficiency of the room temperature ozone decomposition catalyst 7 increases. When the temperature is 50℃, the ozone decomposition efficiency of the room temperature ozone decomposition catalyst 7 is 0.1% lower than that at 46℃. Therefore, when using the room temperature ozone decomposition catalyst 7, the ozone decomposition efficiency is best when the temperature is set to 46℃.

[0119] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A catalyst for room temperature ozone decomposition and a preparation method thereof, characterized in that: The preparation method of the catalyst for normal temperature ozone decomposition is as follows: Step S1, pretreatment and activation of honeycomb ceramics and activated carbon; Step S2, loading the activated carbon onto the honeycomb ceramic carrier; Step S3, pretreatment and activation of the glass fiber filter; Step S4, compounding the glass fiber filter screen with the honeycomb ceramic carrier loaded with activated carbon; Step S5, adding active components; Step S6, performing performance testing on the catalyst for normal temperature ozone decomposition; In S1, the following steps are also included: S11, completely immersing the honeycomb ceramic with a size of 100mm×100mm×100mm in deionized water for 0.5h, rinsing the immersed honeycomb ceramic with deionized water, then putting the rinsed honeycomb ceramic into an ultrasonic cleaning machine, adding deionized water into the ultrasonic cleaning machine, starting the ultrasonic cleaning machine for cleaning for 0.5h, taking the cleaned honeycomb ceramic out of the ultrasonic cleaning machine, and placing the honeycomb ceramic in a drying oven for drying at a drying temperature of 120°C for 2 hours; S12, placing the dried honeycomb ceramic in a high temperature furnace, heating the temperature to 400°C at a heating rate of 5°C / min, and keeping the temperature for 3 hours. After the calcination is completed, the high temperature furnace is naturally cooled to room temperature and the honeycomb ceramic is taken out, and the calcined honeycomb ceramic is immersed in a 1 mol / L nitric acid solution for 1 hour, with continuous stirring during the immersion process. After the acid wash is completed, the honeycomb ceramic is thoroughly rinsed with deionized water until the rinse liquid is neutral, and then the rinsed honeycomb ceramic is placed in a drying oven for drying, and the drying temperature and time are the same as those during the pretreatment; S13, using a sieve to screen the activated carbon to obtain activated carbon with an average particle size of 10 mm, completely immersing the activated carbon in deionized water for 0.5 h, and rinsing the immersed activated carbon with deionized water, then putting the rinsed activated carbon into an ultrasonic cleaning machine, adding deionized water to the ultrasonic cleaning machine until the water level of the deionized water covers the activated carbon, and starting the ultrasonic cleaning machine for cleaning for 0.5 h; The activated carbon was completely immersed in a 1.5 mol / L dilute hydrochloric acid solution for 1 hour. Stirring was continued during the immersion process. After the acid washing was completed, the activated carbon was repeatedly rinsed with deionized water until the rinse liquid was neutral. The rinsed activated carbon was placed in a drying oven for drying at a temperature of 105°C for 2 hours. S14. Place the pretreated activated carbon into a steam activation reactor and start heating it to make the activated carbon reach the required activation temperature, which is 700°C. When the activated carbon reaches the activation temperature, introduce steam and keep the activation time for 2 hours. After the activation is completed, stop heating and introducing steam, allow the steam activation reactor to cool naturally to room temperature, and open the steam activation reactor to collect the activated carbon after steam activation.

2. A catalyst for room temperature ozone decomposition and a preparation method thereof according to claim 1, characterized in that: In S2, the following steps are also included: S21, crushing the activated carbon to obtain activated carbon powder with an average particle size of 1 mm, mixing the activated carbon powder with deionized water to form a uniform loading slurry, adding carboxymethyl cellulose as a binder, immersing the pretreated and activated honeycomb ceramic in the loading slurry, and after soaking for 5 hours, taking out the honeycomb ceramic carrier, and using compressed air to remove excess slurry on the surface; S22, placing the honeycomb ceramic carrier loaded with activated carbon in a drying oven for drying, the drying temperature is 110° C., and the drying time is 4 hours.

3. A room temperature ozone decomposition catalyst and a preparation method thereof according to claim 1, characterized in that: In S3, the following steps are also included: S31, putting a glass fiber filter with a size of 100 mm×100 mm×10 mm into a washing machine, adding a neutral detergent, and washing with deionized water for 20 minutes. After washing, rinse the filter with deionized water for multiple times, and put the rinsed glass fiber filter into a drying machine at a drying temperature of 65° C. for 40 minutes; S32. Fix the glass fiber filter on the workbench of the sandblasting machine for sandblasting. The sandblasting material is white corundum, the sandblasting pressure is 0.5MPa, the sandblasting distance is 100mm, and the sandblasting time is 1.5h. After the sandblasting is completed, use deionized water to clean and dry the glass fiber filter.

4. A catalyst for room temperature ozone decomposition and a preparation method thereof according to claim 1, characterized in that: In S4, the following steps are also included: S41. A layer of acrylic adhesive is uniformly coated on the surface of the honeycomb ceramic carrier loaded with activated carbon, and the pretreated and activated glass fiber filter is covered on the honeycomb ceramic carrier coated with the acrylic adhesive.

5. A room temperature ozone decomposition catalyst and a preparation method thereof according to claim 4, characterized in that: In S4, the following steps are also included: S42, placing the honeycomb ceramic carrier composited with the glass fiber filter and loaded with activated carbon in a vacuum chamber, starting the vacuum pump to form a negative pressure environment, the glass fiber filter will be adsorbed onto the honeycomb ceramic carrier to form a preliminary combination with the acrylic adhesive, and a preliminary composite material is obtained; S43, taking out the preliminary composite material after vacuum adsorption, placing it in a mechanical pressing device, using a roller press to apply uniform pressure to the preliminary composite material, and then placing the preliminary composite material in a hot press to perform hot pressing curing treatment to obtain a complete composite material.

6. A catalyst for room temperature ozone decomposition and a preparation method thereof according to claim 1, characterized in that: In S5, the following steps are also included: S51. Prepare a precursor solution through the active component precursor, immerse the complete composite material in the precursor solution, fix the active component accounting for 10% of the total mass on the complete composite material, take out the complete composite material, dry it at 120°C for 3h, and calcine it at 500°C for 3h to obtain a catalyst for room temperature ozone decomposition.

7. A catalyst for room temperature ozone decomposition and a preparation method thereof according to claim 6, characterized in that: The active component precursor is one or more of 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate and nickel nitrate hexahydrate.

8. A room temperature ozone decomposition catalyst and a preparation method thereof according to claim 1, characterized in that: In S6, the following steps are also included: S61. Precursor solutions are prepared in sequence by 50% manganese nitrate solution, cobalt nitrate hexahydrate, iron nitrate nonahydrate, copper nitrate trihydrate, nickel nitrate hexahydrate, 50% manganese nitrate solution and cobalt nitrate hexahydrate, 50% manganese nitrate solution and iron nitrate nonahydrate, 50% manganese nitrate solution and copper nitrate trihydrate, 50% manganese nitrate solution and nickel nitrate hexahydrate, and are numbered 1-9.

9. A catalyst for room temperature ozone decomposition and a preparation method thereof according to claim 1, characterized in that: In S6, the following steps are also included: S62, immersing the complete composite material in the precursor solution 1-9, fixing the active components accounting for 10% of the total mass on the complete composite material, taking out the complete composite material, drying it at 120° C. for 3 h, and calcining it at 500° C. for 3 h, to obtain the room temperature ozone decomposition catalyst 1-9; At a temperature of 30°C and a space velocity of 10000h -1 , oxygen concentration of 20 vol% and ozone concentration of 100 ppmv, the loading amount of the room temperature ozone decomposition catalyst was 2 g, and the ozone decomposition efficiency of the room temperature ozone decomposition catalysts 1-9 under the same conditions was measured using an Eco Sensors UV-100 ozone analyzer to obtain a group of room temperature ozone decomposition catalysts with the highest ozone decomposition efficiency.

10. A catalyst for room temperature ozone decomposition and a preparation method thereof according to claim 1, characterized in that: In S6, the following steps are also included: S63, a group of room temperature ozone decomposition catalysts with the highest ozone decomposition efficiency is heated at a space velocity of 10000 h -1 Under the conditions of oxygen concentration of 20 vol% and ozone concentration of 100 ppmv, the ozone decomposition efficiency at temperatures of 30°C, 34°C, 38°C, 42°C, 46°C and 50°C was measured using an Eco Sensors UV-100 ozone analyzer.

Citation Information

Patent Citations

  • Porous active carbon composite material and manufacturing method thereof

    CN101259404A

  • Regular honeycomb ceramic carbon carrier based doped ozone catalyst for advanced treatment of industrial wastewater and preparation method of regular honeycomb ceramic carbon carrier based doped ozone catalyst

    CN106390988A

  • Honeycomb ceramic-porous carbon monolithic catalyst, honeycomb ceramic-porous carbon monolithic adsorbent, and preparation method and application of monolithic adsorbent

    CN111495410A

  • Catalytic denitration heat accumulator

    CN115999534A

  • Three-way catalyst with activated carbon filter screen convenient to replace

    CN210564718U