High-loading-capacity Ru monatomic catalyst 4RuCeO2-AA as well as preparation method and application thereof

By designing defects on CeO2 support and loading Ru ions by impregnation method, a high-load Ru single-atom catalyst 4RuCeO2-AA is formed, which solves the problems of low loading and poor stability of precious metal single-atom catalysts in the prior art, and achieves high-efficiency catalysis The activity and stability of chlorine oxide benzene are improved.

CN118988304APending Publication Date: 2024-11-22TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411026464.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the use of metal oxides as support to synthesize high-load precious metal single-atom catalysts is challenged, especially in terms of stability and activity, and the precious metal loading is low.

Method used

By designing defects on CeO2 support, using ascorbic acid treatment to make it CeO2-AA, loading Ru ions by impregnation method to form a high-loaded Ru single-atom catalyst 4RuCeO2-AA, ensuring that Ru ions exist in a highly dispersed form and improving catalytic activity and stability.

Benefits of technology

Under the same loading, 4RuCeO2-AA significantly improves catalytic activity and stability, and can efficiently catalyze chlorobenzene oxidation at lower temperatures, maintaining a 99% conversion rate for more than 20 hours, while the activity of traditional 4RuCeO2 catalysts decreases under the same conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988304A_ABST
    Figure CN118988304A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical catalyst synthesis and application thereof, and provides a high-loading-capacity Ru monatomic catalyst 4RuCeO2-AA and a preparation method and application thereof, CeO2 is used as a carrier, the CeO2 carrier has a large number of defect CeO2-AA through defect design, and Ru ions accounting for 4 wt% of the total mass of the carrier are still in an atomic-scale dispersion state after being loaded on CeO2-AA through impregnation. The catalyst 4RuCeO2-AA is formed by combining noble metal Ru with a CeO2 carrier CeO2-AA treated by ascorbic acid, ascorbic acid enables more oxygen vacancies and Ce < 3 + > to be generated in CeO2 so as to anchor Ru monatomic, structural defects are utilized to coordinate with the monatomic so as to stabilize the monatomic, and the monatomic is highly dispersed and loaded on the carrier. At a relatively low temperature of 240 DEG C, the conversion rate of the p-chlorobenzene can be kept at 99%, and the p-chlorobenzene is not inactivated after lasting for 20 hours. The result shows that the 4RuCeO2-AA has good activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of chemical catalyst synthesis and application thereof, and specifically relates to a high-loaded Ru single-atom catalyst 4RuCeO2-AA and a preparation method and application thereof, and application of the catalyst in catalytic oxidation of chlorinated volatile organic compounds (CVOCs). Background Art

[0002] Volatile organic compounds (VOCs) are the first to be affected. Among them, chlorinated volatile organic compounds (CVOCs) are the most noteworthy type of pollutants, because chlorinated chemicals are an important part of modern industrial manufacturing raw materials. Due to technical limitations, a large amount of CVOCs emissions will inevitably be generated in the production chain. They are more chemically stable, more toxic, and more difficult to degrade. The catalytic oxidation method with high-efficiency catalysts as the core is considered to be the most promising terminal treatment strategy for completely eliminating CVOCs (represented by chlorobenzene (CB)). It has low operating temperature, low energy consumption, high efficiency, and no secondary pollution.

[0003] Designing and developing efficient catalysts is the key to catalytic oxidation technology. Currently, single atom catalysts (SACs) have become the most active part of the catalytic field due to their excellent catalytic activity. Ru SACs have shown excellent performance in many catalytic applications due to their high atomic utilization efficiency and catalytic activity. Through the interaction between metal carriers, single atoms are stabilized to achieve atomic-level dispersion.

[0004] For Ru SACs single-atom catalysts, the first experimental study only appeared in the literature in 2017. 3+ ) stabilizes Ru single atoms. So far, most of the carriers used to stabilize Ru single atoms are based on carbon materials, including activated carbon, N-doped carbon, N-doped graphene and carbonitride, and the loading of single-atom Ru on γ-graphene can reach 27.8 wt %. However, there are still relatively few examples of metal oxides as carriers to load single noble metal atoms. In previous studies, there have been Au (0.5 wt%) catalysts loaded with single-atom dispersion on ceria carriers, Pt (1.0 wt%) single-atom catalysts, and Ru (1.0 wt%) catalysts loaded with atomic dispersion by hydrothermal method, but the loading of noble metals in these single-atom catalysts is low and does not exceed 1.0 wt %. These studies all show that the use of metal oxides as carriers to synthesize high-load noble metal single-atom catalysts still faces challenges. Summary of the invention

[0005] The present invention provides a high-loaded Ru single-atom catalyst 4RuCeO2-AA and a preparation method and application thereof. CeO2 is used as a carrier, and a large number of defects are made to the CeO2 carrier through defect design (CeO2-AA). Then, through an impregnation method, 4% of the total mass of the carrier is loaded on the CeO2-AA, and the Ru ions are still in an atomic-level dispersed state (4RuCeO2-AA).

[0006] When the same mass fraction of Ru ions was loaded in the same way, the CeO2 carrier in the reference catalyst 4RuCeO2 was not defect-treated. When the mass dispersion of Ru was 4%, the Ru species existed in the form of RuO2 nanoparticles.

[0007] The Ru species in the two catalysts have different forms, and their activity and stability for the catalytic oxidation of CVOCs are quite different. CB was selected as the target pollutant, and its catalytic activity and stability were verified by short-time temperature rise activity test and fixed temperature stability test. The results show that 4RuCeO2-AA is superior to 4RuCeO2 in both activity and stability. Analysis of its dispersion and acidic sites by CO-TPD and NH3-TPD showed that its activity comes from the increase in active sites brought about by the single-atom dispersion form, while the increase in stability is due to the increase in the number of strong acid sites, which are conducive to the dissociation and deep oxidation of CB.

[0008] The present invention is realized by the following technical scheme: a high-loaded Ru single-atom catalyst 4RuCeO2-AA, wherein the catalyst 4RuCeO2-AA is a combination of precious metal Ru and a CeO2 carrier CeO2-AA treated with ascorbic acid, and ascorbic acid causes defects in CeO2 to capture Ru 3+ It is loaded on the carrier in a highly dispersed form.

[0009] At the same precious metal loading, the highly dispersed form provides more active sites for the catalytic reaction, improving the activity of the catalyst in catalytic oxidation of CB; at the same time, it also increases the number of strong acid sites of the catalyst, which is beneficial to the dissociation and deep oxidation of CB, and increases the stability of the catalyst in catalytic oxidation of CB.

[0010] The method for preparing the high-loaded Ru single-atom catalyst 4RuCeO2-AA comprises the following steps: (1) Preparation of CeO2: 0.01 mol of cerium nitrate hexahydrate was mixed with 100 ml of deionized water, stirred vigorously for 30 min, ammonia water was added to adjust the pH to 9.5, stirring was continued for 3 h, the mixture was allowed to stand overnight, the precipitate was filtered and repeatedly washed until neutral, dried in a 100°C forced air oven for 8 h, then heated to 400°C at a heating rate of 5°C / min and kept for 4 h. The solid powder obtained after natural cooling was CeO2. (2) 0.5 g of the CeO2 solid powder synthesized in step (1) was dispersed in 50 mL of deionized water and stirred for 30 min, which was recorded as solution A. 0.5 mmol of ascorbic acid was dissolved in 50 mL of deionized water and stirred for 30 min, which was recorded as solution B. Solution B was slowly added to solution A, and the mixed solution was stirred vigorously for 1 h. The deionized water was centrifuged and washed 4 times, each time at 4000 r / min for 10 min. The precipitate was re-dispersed in 50 ml of deionized water, and 20.5254 mL of 2 mg / mL ruthenium chloride solution was added. The mixture was immersed and stirred for 2 h to load the Ru species, and then stirred at 80 °C until the solvent was evaporated. The obtained product was dried at 100 °C for 12 h, and then heated to 350 °C at a heating rate of 5 °C / min and calcined in air for 2 h. The solid powder obtained after natural cooling was 4RuCeO2-AA with a Ru loading of 4 wt%.

[0011] The present invention also provides the use of the high-loaded Ru single-atom catalyst 4RuCeO2-AA or the 4RuCeO2-AA prepared by the method in the catalytic oxidation of chlorobenzene CVOCs.

[0012] The 4RuCeO2-AA catalyst is used as a catalyst in the catalytic oxidation of chlorobenzene CVOCs at ≤240°C.

[0013] The 4RuCeO2-AA catalyst obtained in the present invention can maintain a chlorobenzene conversion rate of 99% for 20 hours without deactivation at a relatively low temperature of 240°C, while the conversion rate of 4RuCeO2 to chlorobenzene is 90%, and its activity continues to decrease with time. The results show that 4RuCeO2-AA has good activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 are transmission electron microscopy (TEM) images of the catalysts synthesized in Examples 3 and 4 of the present invention, wherein Figures (a) and (b) are CeO2 synthesized in Example 3, and Figures (c) and (d) are CeO2-AA synthesized in Example 4; Figure 2are spherical aberration corrected high angle annular dark field scanning transmission microscope (AC-HAADF-STEM) images of the catalysts synthesized in Examples 3 and 4 of the present invention, wherein Figures (a), (b) and (c) are 4RuCeO2, and Figures (d), (e) and (f) are RuCeO2-AA; Figure 3 The X-ray diffraction patterns (XRD) of the catalysts CeO2, CeO2-AA, 4RuCeO2 and 4RuCeO2-AA synthesized in Examples 1, 2, 3 and 4 of the present invention; Figure 4 is the Ru 3p orbital X-ray photoelectron spectrum (XPS) of the catalysts synthesized in Examples 3 and 4 of the present invention; Figure 5 1 is a curve of chlorobenzene conversion and CO2 mineralization rate of the catalysts synthesized in Examples 1, 2, 3 and 4 of the present invention, wherein the initial concentration of chlorobenzene is 500 ppm and the space velocity is 15000 mL / (gh); in the figure, the left figure is the chlorobenzene conversion rate, and the right figure is the CO2 mineralization rate curve; Figure 6 This is a durability test curve of the catalyst synthesized in Examples 3 and 4 of the present invention under the reaction conditions described in Example 5, wherein the initial chlorobenzene concentration is 500 ppm, the space velocity is 15000 mL / (gh), the reaction temperature is 240°C, and the reaction time is 20 h. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0016] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and the disclosure and materials cited therein are hereby incorporated by reference.

[0017] Technical equivalents to the specific embodiments described that are apparent to those skilled in the art using no more than routine experimentation are intended to be encompassed by this application.

[0018] The experimental methods in the following examples are all conventional methods unless otherwise specified. The instruments and equipment used in the following examples are all conventional laboratory instruments and equipment unless otherwise specified; the experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.

[0019] Example 1: Preparation of CeO2 carrier: First, 0.01 mol (4.3422 g) of cerium nitrate hexahydrate (99.5%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) and 100 mL of deionized water were mixed and stirred vigorously for 30 min. Ammonia water (25%, purchased from Tianjin Tianli Chemical Reagent Co., Ltd.) was added to adjust the pH to 9.5. Stirring was continued for 3 h. The mixture was allowed to stand overnight. The precipitate was filtered and washed repeatedly until it was neutral. The mixture was dried in a 100°C forced air oven for 8 h. The mixture was then placed in a tubular furnace and heated to 400°C (heating rate of 5°C / min) with air and maintained for 4 h. The obtained solid powder was recorded as CeO2.

[0020] Example 2: Preparation of CeO2-AA carrier: Take 0.5g of the CeO2 solid powder synthesized in Example 1, disperse it in 50mL of deionized water, stir for 30min, and record it as solution A. Then, 0.5mmol (0.08806g) of ascorbic acid (>99.0%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.) was dissolved in 50mL of deionized water and stirred for 30min, which was recorded as solution B. Solution B was slowly added to solution A, and the mixed solution continued to be vigorously stirred for 1h, centrifuged and washed 4 times (each time at 4000r / min for 10min), and the precipitate was re-dispersed in 50ml of deionized water. After stirring for 2h, the temperature was raised to 80℃ until the solvent was evaporated; the product was placed in a 100℃ forced air drying oven and dried for 12h, and calcined in air at 350℃ in a tubular furnace for 2h (heating rate of 5℃ / min), and finally the obtained solid powder was recorded as CeO2-AA.

[0021] Example 3: Preparation of 4RuCeO2 catalyst: Take 0.5 g of the solid powder CeO2 synthesized in Example 1, disperse it in 50 mL of deionized water, stir for 2 h, add 20.5254 mL of the prepared ruthenium chloride solution, immerse and stir for 2 h, then stir at 80°C until the solvent is evaporated, put it into a forced air drying oven at 100°C for 12 h, and calcine it in air at 350°C in a tubular furnace for 2 h (heating rate of 5°C / min), and finally record the obtained solid powder as 4RuCeO2 (Ru loading 4 wt%).

[0022] Example 4: Preparation of 4RuCeO2-AA catalyst: 0.5 g of CeO2 solid powder synthesized in Example 1 was dispersed in 50 mL of deionized water and stirred for 30 min, which was recorded as solution A. Then 0.5 mmol (0.08806 g) of ascorbic acid was dissolved in 50 mL of deionized water and stirred for 30 min, which was recorded as solution B. Solution B was slowly added to solution A, and the mixed solution was stirred vigorously for 1 h. The mixed solution was washed by centrifugation 4 times (each time at 4000 r / min for 10 min), and the precipitate was removed. The material was redispersed in 50 ml of deionized water, and then 20.5254 mL of prepared ruthenium chloride solution (99.95%, purchased from Tianjin Xiensiopude Technology Co., Ltd., with a concentration of 2 mg / mL) was added, and the mixture was immersed and stirred for 2 h to load the Ru species. Then, the mixture was stirred at 80 °C until the solvent was evaporated, dried in a forced air drying oven at 100 °C for 12 h, and calcined in a tubular furnace at 350 °C in air for 2 h (heating rate of 5 °C / min). Finally, the obtained solid powder was recorded as 4RuCeO2-AA (Ru loading 4 wt%).

[0023] Example 5: The activity and stability of the catalyst are completed by connecting a fixed bed reactor to a gas chromatograph equipped with 2 FID detectors and a nickel converter. 100 mg of sample (40-60 mesh) is placed in a quartz tube with an inner diameter of 8 mm, and the catalyst is stabilized by quartz sand and quartz wool before and after. The gas flows from the upper part of the quartz tube to the lower part, and the temperature of the catalyst bed is measured by inserting a thermocouple into the quartz tube from the top. Chlorobenzene gas is obtained by volatilization of liquid chlorobenzene. The volatilization amount is adjusted by a set of cooling circulation equipment, and the concentration and air velocity of chlorobenzene are adjusted by the flow rate of air. The initial concentration of chlorobenzene is 500ppm, the total flow rate is 25 mL, and the air velocity is 15000 mL / (gh). The chlorobenzene concentration is measured by the FID detector, and CO2 is detected by FID in conjunction with the nickel converter.

[0024] Figure 1 are the HR-TEM images of the catalysts synthesized in Examples 1 and 2. Figure 1 It can be seen that both CeO2 and CeO2-AA catalysts are regular and smooth ellipsoidal in shape, with similar size and shape, indicating that the ascorbic acid treatment has no effect on the macroscopic morphology of the catalyst support. It can be inferred that the difference in activity after the support is loaded with the precious metal Ru may come from the change in its surface physicochemical properties.

[0025] Figure 2 The AC-HAADF-STEM images of the catalysts synthesized in Examples 3 and 4 are shown in Figure 1. Figure 2It can be seen that atomically dispersed noble metal Ru species are evenly distributed on the surface of CeO2 or CeO2-AA catalysts, indicating that we have successfully synthesized Ru-based single-atom dispersed catalysts. Figure 2 (c) Ru species with nanocluster morphology. In order to further analyze the phase of Ru species, XRD characterization is required.

[0026] Figure 3 It is the XRD spectrum of the catalysts synthesized in Examples 1, 2, 3 and 4. It can be seen from the figure that all four catalysts present CeO2 crystal structure; compared with CeO2 and CeO2-AA carriers, after loading Ru species, the peak intensity of CeO2 crystal phase in 4RuCeO2 and 4RuCeO2-AA catalysts becomes weaker, indicating that the loading of precious metals can cause more defects in the catalysts, but the degree of weakening of the two is similar, indicating that the change of defect sites may not be the main reason for their activity differences; both catalysts have been calcined in high-temperature air, and the loaded Ru species will be converted into RuO2. After careful observation, it is found that the diffraction peaks belonging to RuO2 species appear at 35.1° and 54.5° in the XRD spectrum of 4RuCeO2 catalyst, while they are not seen on the surface of 4RuCeO2-AA, indicating that RuO2 species are more dispersed in 4RuCeO2-AA catalyst, mainly because the ascorbic acid-treated carrier CeO2-AA can make RuO2 more dispersed, which may be the main source of its activity.

[0027] Figure 4 3p-XPS spectra of the catalysts synthesized in Examples 3 and 4. The peaks at the binding energies of 486.0 and 463.0 eV in the spectra are respectively attributed to Ru 3p 1 / 2 and Ru 3p 3 / 2 orbital, corresponding to RuO2 species; in addition, the peak area fitting calculation proves that the peak areas are the same, indicating that the content of Ru species is similar, so the sources of the two catalysts 4RuCeO2 and 4RuCeO2-AA are likely to be caused by different dispersions. According to the XRD results, 4RuCeO2-AA has higher dispersion, which may be the reason for its high activity.

[0028] Figure 5It is the chlorobenzene conversion rate and CO2 mineralization rate curve of the catalyst synthesized in Examples 1, 2, 3 and 4. It can be seen that the activity of CeO2 and CeO2-AA carriers is poor, and there are two fluctuations in the activity curve, which is due to the Cl species covering the active site, resulting in its inactivation, but the temperature corresponding to the fluctuation of the carrier CeO2-AA after ascorbic acid treatment is significantly reduced, and the conversion rate will continue to rise after 300°C. After loading 4 wt% of Ru species, the chlorobenzene conversion rate and CO2 mineralization rate of the formed catalysts 4RuCeO2 and 4RuCeO2-AA are greatly improved, and 4RuCeO2-AA is more active, and it has been completely converted at 240°C, and at the same temperature, its CO2 mineralization rate is also significantly higher than 4RuCeO2. Combined with the results of TEM, XRD and XPS, the better activity of 4RuCeO2-AA is likely to be caused by higher dispersion.

[0029] Figure 6 The catalytic stability curves of the catalysts synthesized in Examples 3 and 4 in chlorobenzene are shown in FIG. 1 . As can be seen from the figure, at a relatively low temperature of 240°C, the conversion rate of chlorobenzene by 4RuCeO2-AA can be maintained at 99% for 20 h without deactivation, while the conversion rate of chlorobenzene by 4RuCeO2 is 90%, and its activity continues to decrease to 78% over time. The results show that 4RuCeO2-AA has good activity and stability.

[0030] Table 1 shows the temperatures corresponding to the conversion rates of chlorobenzene catalyzed by the catalysts synthesized in Examples 3 and 4 of the present invention when the conversion rates are 50%, 90% and 100%; T 50 , T 90 and T 100 The temperatures corresponding to the conversion rates of chlorobenzene in catalytic oxidation are 50%, 90% and 100%, respectively. The table lists the temperatures corresponding to 50%, 90% and 100% conversion rates of chlorobenzene catalytic oxidation of 4RuCeO2-AA and 4RuCeO2 catalysts. It can be seen that when the conversion rate is 50%, the temperature difference between the two catalysts is 10°C. The conversion rate of 4RuCeO2-AA reaches 90% at 215°C and is completely converted at 240°C, while 4RuCeO2 only reaches 90% at 240°C and can be completely converted at 280°C.

[0031] Table 1: T corresponding to the catalytic oxidation of chlorobenzene by the synthesized catalysts of Examples 3 and 4 of the present invention 50 , T 90 and T 100 , where the initial chlorobenzene concentration is 500 ppm and the space velocity is 15000 mL / (gh) Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high-loaded Ru single-atom catalyst 4RuCeO2-AA, characterized in that: The catalyst 4RuCeO2-AA is a combination of precious metal Ru and CeO2 carrier CeO2-AA treated with ascorbic acid. Ascorbic acid causes defects in CeO2 to capture Ru. 3+ It is loaded on the carrier in a highly dispersed form at the atomic level.

2. A method for preparing the high-loaded Ru single-atom catalyst 4RuCeO2-AA according to claim 1, characterized in that: The steps include: (1) Preparation of CeO2: 0.01 mol of cerium nitrate hexahydrate was mixed with 100 ml of deionized water, stirred vigorously for 30 min, ammonia water was added to adjust the pH to 9.5, stirring was continued for 3 h, and the mixture was allowed to stand overnight. The precipitate was filtered and washed repeatedly until it was neutral, and dried in a 100 °C forced air oven for 8 h, and then heated to 400 °C at a heating rate of 5 °C / min and kept reacting for 4 h. The solid powder obtained after natural cooling was CeO2. (2) 0.5 g of the CeO2 solid powder synthesized in step (1) was dispersed in 50 mL of deionized water and stirred for 30 min, which was recorded as solution A. 0.5 mmol of ascorbic acid was dissolved in 50 mL of deionized water and stirred for 30 min, which was recorded as solution B. Solution B was slowly added to solution A, and the mixed solution was stirred vigorously for 1 h. The deionized water was centrifuged and washed 4 times, each time at 4000 r / min for 10 min. The precipitate was re-dispersed in 50 ml of deionized water, and 20.5254 mL of 2 mg / mL ruthenium chloride solution was added. The mixture was immersed and stirred for 2 h to load the Ru species, and then stirred at 80 °C until the solvent was evaporated. The obtained product was dried at 100 °C for 12 h, and then heated to 350 °C at a heating rate of 5 °C / min and calcined in air for 2 h. The solid powder obtained after natural cooling was 4RuCeO2-AA with a Ru loading of 4 wt%.

3. Use of the high-loaded Ru single-atom catalyst 4RuCeO2-AA according to claim 1 or the 4RuCeO2-AA prepared by the method according to claim 2 in the catalytic oxidation of chlorobenzene CVOCs.

4. The use according to claim 3, characterized in that: The 4RuCeO2-AA catalyst is used as a catalyst in the catalytic oxidation of chlorobenzene CVOCs at ≤240°C.

5. The use according to claim 4, characterized in that: The initial concentration of chlorobenzene is 500 ppm, the total flow rate is 25 mL, and the space velocity is 15000 mL / (gh); the amount of the 4RuCeO2-AA catalyst is 100 mg; the conversion rate of 4RuCeO2-AA for chlorobenzene is maintained at 99% and is not deactivated for 20 hours.

Citation Information

Patent Citations

  • Preparation method of monoatomic catalyst for indoor air purification

    CN106622227A

  • Monoatomic catalyst as well as preparation and application thereof

    CN109954489A

  • Flaky atomic-scale Pt / CeO2 catalyst with ultrahigh Pt loading capacity and preparation method of flaky atomic-scale Pt / CeO2 catalyst

    CN114832817A

  • Cu1 / CeO2 monatomic catalyst and preparation method thereof

    CN117884136A

  • Preparation method and application of Ru monatomic noble metal type catalyst RuCeTi

    CN118179502A