Preparation method and application of MOF-derived ferrocobalt composite material

By calcining the MOF-derived cobalt-iron composite material CoFeCMs (CO2) prepared under a mild oxidation atmosphere of CO2, the problems of insufficient active sites and poor stability of MOF-derived cobalt materials were solved, and the effect of efficient degradation ofofloxacin was achieved.

CN118988320AActive Publication Date: 2024-11-22YANGTZE ECOLOGY & ENVIRONMENT CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411100339.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing MOF-derived cobalt materials have problems of insufficient active sites and poor stability during the catalytic antibiotic degradation process, making it difficult to effectively remove ofloxacin antibiotics in water.

Method used

Fe-ZIF 67 was prepared by co-precipitation method, and then calcined under a mild oxidation atmosphere of CO2 to prepare MOF-derived cobalt-iron composite CoFeCMs (CO2). This material has a relatively complete carbon framework and rich bimetallic active sites, which improves the Catalytic properties.

Benefits of technology

The degradation rate of ofloxacin reached 94.2% within 30 minutes, significantly improving the catalytic performance and stability, providing more active sites and excellent electron transfer efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988320A_ABST
    Figure CN118988320A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an MOF-derived ferrocobalt composite material. Fe-ZIF 67 of a dodecahedron structure is synthesized through a coprecipitation method, and then the ferrocobalt composite material is synthesized through carbonization and oxidation two-step calcination. Under the mild CO2 atmosphere, the loss of a carbon skeleton of ZIF in the oxidation process is small, the MOF-derived ferrocobalt bimetallic composite material CoFeCMs (CO2) prepared through calcination has a larger specific surface area and a complete carbon skeleton, more active sites are provided, meanwhile, more excellent catalytic performance and electron transfer efficiency are achieved, and the efficiency of CoFeCMs (CO2) for activating PMS to degrade OFX within 30 min can reach 94.2%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibiotic treatment of organic matter pollution, and specifically to a preparation method and application of a MOF-derived cobalt-iron composite material. Background Art

[0002] Antibiotics are widely used in medicine and veterinary medicine as compounds with antibacterial, antiviral and antifungal activities. Antibiotics can enter the environment through various pathways, such as the pharmaceutical industry, hospital sewage, and the disposal of human and animal waste. About 30-90% of antibiotics remain active and are not metabolized and are excreted into the environment through urine and feces, which may lead to the development of antibiotic-resistant pathogens, thus potentially threatening ecosystems and human health. Traditional biological treatment methods have difficulty in effectively removing recalcitrant antibiotics from water bodies because antibiotics are highly toxic to bacterial communities, which can cause the biological process of wastewater treatment to stop.

[0003] Ofloxacin OFX is a third-generation fluoroquinolone antibiotic that can be frequently detected in water bodies. The concentration of OFX detected in local water bodies in eastern my country was as high as 254.74 ng / L, which is much higher than other antibiotics.

[0004] MOF-derived materials retain the advantages of MOF materials such as three-dimensional pore structure, large specific surface area, abundant active sites, adjustable metal elements and pore structure, and are a promising SR-AOPs catalyst. Advanced oxidation technology based on sulfate radicals SR-AOPs has excellent mineralization rate and applicability for antibiotics and other refractory organic matter. The SR-AOPs method mainly produces SO4 ·- and ·OH strong oxidizing species, whose reduction potentials (E) are 2.8 V and 2.5-3.1 V, respectively, which can rapidly and non-selectively oxidize antibiotic pollutants in wastewater.

[0005] Cobalt is considered to be the most effective transition metal for SR-AOPs to remove organic pollutants. However, the catalytic performance of MOF-derived cobalt-based metal materials is limited, and they are prone to agglomeration and have poor stability. 3+ / Co 2 + , Fe 3+ / Fe 2+ However, the cobalt-iron bimetallic materials derived from MOFs are limited by the low number of active sites and the easy leaching of metal ions, which restricts their application, and their activity and stability need to be further improved. Summary of the invention

[0006] The purpose of the present invention is to provide a preparation method and application of a MOF-derived cobalt-iron composite material, wherein the prepared MOF-derived cobalt-iron bimetallic composite material is calcined in a CO2 mild oxidizing atmosphere, and the prepared MOF-derived cobalt-iron composite material has a relatively complete carbon skeleton and abundant bimetallic active sites, thereby improving the catalytic performance. The composite material can be applied to activate peroxymonosulfate to degrade ofloxacin.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] A method for preparing a MOF-derived cobalt-iron composite material comprises the following steps:

[0009] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0010] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0011] Take 0.67-0.8mL of 0.8mol / L Co(NO3)2·6H2O and 9.6-10.7mL of 0.1mol / L FeCl3·6H2O solution and mix them evenly, dilute them to 12mL with water, and use them as solution B after ultrasonic treatment for 10min. The molar ratio of Co element to Fe element in solution B is 1:1.5-2;

[0012] Solution B was slowly added dropwise to solution A under stirring. After the addition was completed, stirring was continued at room temperature for 24 h. The mixture was centrifuged to collect the solids. The solids were then repeatedly washed with water and methanol alternately for several times and dried at 60 °C to obtain the precursor Fe-ZIF 67.

[0013] Step 2: Carbonization to prepare CoFe@C:

[0014] The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat in a tube furnace, heated to 500-800°C, and kept warm for 2 hours under Ar atmosphere to obtain CoFe@C;

[0015] Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2):

[0016] The CoFe@C prepared in step 2 is placed in a tubular furnace, the temperature is raised to 500°C, a continuous flow of CO2 is introduced into the tubular furnace as a gas atmosphere, and the temperature is kept for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

[0017] Preferably, the heating rate of the tube furnace in step 2 is 5°C / min.

[0018] Preferably, the heating rate of the tube furnace in step three is 5°C / min.

[0019] Preferably, the centrifugal speed of the mixed solution in step 1 is 8000 rpm.

[0020] The invention discloses an application of a MOF-derived cobalt-iron composite material, wherein the MOF-derived cobalt-iron composite material is applied to activate peroxymonosulfate to degrade ofloxacin.

[0021] Preferably, the MOF-derived cobalt-iron composite material is used to activate peroxymonosulfate to degrade ofloxacin. The degradation method is as follows: 100 mL of OFX solution with a concentration of 20 mg / L is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.4 g of MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS are added to the beaker, and PMS is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to degrade OFX; the degradation time is 30 min, 2-3 mL of the solution in the degradation process is taken out with a syringe, the solution is filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette, and the OFX concentration is analyzed by UV-Vis at a wavelength of 294 nm, and the degradation rate of OFX is 94.2%.

[0022] Characterization of the MOF-derived cobalt-iron composite material CoFeCMs(CO2) prepared in the present invention:

[0023] 1. Characterization of microscopic morphology

[0024] CoFeCMs(CO2) and precursors were characterized by electron microscopy, such as Figure 2 As shown in (a), the synthesized Fe-ZIF67 has a dodecahedral structure. Figure 2 (b) is CoFe@C formed by carbonization. It can be seen that the surface of CoFe@C becomes rough, but the morphology is similar to that of Fe-ZIF 67. Figure 2 As can be seen from (c), (e) and (f), the surface of CoFeCMs(CO2) formed by oxidation of CoFe@C in a CO2 atmosphere is rough, but the surface of the dodecahedron is slightly concave, which is caused by the collapse of the carbon skeleton of ZIF during the oxidation process, while CoFeCMs(CO2) still retains most of the carbon skeleton; in contrast, Figure 2(d) The dodecahedral structure of CoFeCMs(air) formed by oxidation of CoFe@C in air atmosphere is destroyed to form agglomerated nanoparticles; the lattice spacing of 0.254nm in HRTEM corresponds to the (311) crystal plane of CoFe2O4. Based on the above analysis, it is confirmed that CO2, as a mild oxidizing atmosphere, can not only generate CoFe2O4, but also protect the loss of carbon skeleton.

[0025] 2. XRD analysis

[0026] Figure 3 (a) is the XRD spectrum of ZIF 67 and its precursor Fe-ZIF 67. It can be seen that the characteristic peaks of Fe-ZIF 67 are consistent with those of ZIF 67, indicating that the crystal structures of Fe-ZIF 67 and ZIF 67 are the same. There are two main characteristic diffraction peaks in CoFe@C, located at 44.3° and 44.7° respectively. The diffraction peak at 44.3° belongs to the (111) plane of elemental cobalt, and the diffraction peak at 44.7° belongs to the (110) plane of elemental iron. The precursor Fe-ZIF 67 was calcined in two steps to obtain CoFeCMs(air), and the characteristic diffraction peaks appeared at 30.3°, 35.7°, 37.3°, 43.5°, 57.2°, and 62.7°, pointing to the (220), (311), (222), (400), (511), and (440) crystal planes of spinel CoFe2O4 (JCPDS No.01-1121). The (220), (311), (222), (400), (511), and (440) crystal planes of spinel CoFe2O4 also appeared in the XRD of CoFeCMs(CO2), proving that CoFe2O4 was synthesized by calcination in a CO2 atmosphere. In addition, the characteristic peaks of zero-valent iron and zero-valent cobalt also appeared in the XRD spectrum of CoFeCMs(CO2), indicating that iron and cobalt were not completely oxidized.

[0027] 3. XPS analysis

[0028] XPS spectroscopy was used to analyze the chemical state and surface element composition of CoFeCMs(CO2) materials, such as Figure 4 As shown in (a), the precursor Fe-ZIF 67 was calcined in a CO2 atmosphere to form CoFeCMs (CO2). The coexistence of C, O, Fe and Co elements was observed in the full spectrum, proving that a composite material containing cobalt iron oxide was successfully prepared in a CO2 atmosphere. In order to further study the surface chemical state of the material, the CoFeCMs (CO2) was subjected to XPS fine spectral analysis. Figure 4 (b) is the detailed XPS image of C1s. The three peaks at 284.8 eV, 285.8 eV and 289.9 eV correspond to the peaks of -CC, -CO and OCO, respectively. Figure 4 (c) shows that CoFeCMs(CO2) at 530.1eV, 531.9eV, and 534.0eV belong to lattice oxygen, adsorbed oxygen, and surface adsorbed water, respectively. The characteristic peak of lattice oxygen at 530.1eV is related to Fe-O / Co-O, and the peak at 531.9eV comes from the CO peak, which corresponds to 285.8eV in the C1s spectrum. It may be that the carbon skeleton of MOF has been partially oxidized. Figure 4 (d) The four peaks are at 706.8 eV, 709.4 eV, 712.9 eV, and 716.83 eV, respectively. The peak at 706.8 eV corresponds to zero-valent iron, and the peaks at 709.4 eV and 712.9 eV are Fe 2+ and Fe 3+ 2p 3 / 2 , the peak at 716.83 eV is a satellite peak; Figure 4 In (e), the peaks at 780.2eV / 795.3 and 782.8eV / 797.9eV of the Co 2p spectrum are Co 2+ (2p 3 / 2 / 2p 1 / 2 ) and Co 3+ (2p 3 / 2 / 2p 1 / 2 ), the peaks at 787.4eV and 803.7 are satellite peaks. Combined with the results of XRD analysis, it can be seen that the method of the present invention successfully prepared CoFeCMs (CO2).

[0029] 4. Raman analysis

[0030] Figure 5 The Raman spectra of Fe-ZIF 67, CoFe@C, CoFeCMs(air) and CoFeCMs(CO2) show the graphitization degree and carbon hybridization orbital type of Fe-ZIF 67, CoFe@C, CoFeCMs(air) and CoFeCMs(CO2). -1 and 1580cm -1 The D band associated with the carbon atom crystal defect and the sp band associated with the carbon atom can be observed at 2 The ratio between the hybridization-related G band, D band and G band is I D / I G The intensity relationship between the two peaks can be described. The precursor Fe-ZIF 67 was not carbonized, so no carbon peak appeared. The carbonized CoFe@C showed D band and G band, indicating the presence of graphitic carbon in CoFe@C. No carbon peak was detected in CoFeCMs(air) calcined in air, indicating that carbon was completely decomposed during the calcination process. CoFeCMs(CO2) calcined in carbon dioxide atmosphere retained the carbon peak in CoFe@C. The I D / IG The values ​​of 1.08 and 1.28 respectively indicate that the graphitization degree of CoFeCMs(CO2) is high and there are obvious crystal defects in the carbon structure. Combined with XRD analysis, CO2 atmosphere is a mild oxidizing atmosphere, which can effectively reduce the loss of carbon skeleton in Fe-ZIF 67. The formed CoFeCMs(CO2) has a more complete carbon skeleton than CoFeCMs(air).

[0031] 5. N2 adsorption curve and BET analysis

[0032] Table 1 records the BET test data of CoFe@C, CoFeCMs(air) and CoFeCMs(CO2). Figure 6 (a) and Table 1 show that the specific surface area of ​​CoFe@C, CoFeCMs (air) and CoFeCMs (CO2) is 46.372 m 2 / g, 9.626m 2 / g, 44.460m 2 / g, the surface area of ​​CoFeCMs(CO2) is much larger than that of CoFeCMs(air), which indicates that the CoFeCMs(CO2) composite catalyst has more active sites. Figure 3-6 (a) shows that the N2 adsorption-desorption isotherms of CoFe@C, CoFeCMs(air) and CoFeCMs(CO2) present type IV isotherms with H3-type hysteresis loops, indicating the existence of mesoporous structures inside the samples. Figure 6 (b) shows that the pore sizes of CoFe@C, CoFeCMs(air) and CoFeCMs(CO2) are mainly mesopores with a diameter of 5 nm. The pore volume of CoFeCMs(CO2) is larger than that of CoFeCMs(air), as shown in Table 1, which is more conducive to the transfer and diffusion of pollutants.

[0033] Table 1

[0034]

[0035] Verification of the catalytic degradation experiment of OFX by CoFeCMs (CO2) prepared in the present invention in activated PMS:

[0036] Calculation formula for target pollutants:

[0037] Among them, R t represents the degradation rate at time t, C0 and C t They represent the initial concentration of the pollutant and the pollutant concentration at time point t respectively.

[0038] The above degradation experiments were repeated three times, and the final experimental results were taken as the mean ± standard deviation.

[0039] 1. Effect of Cobalt-Iron Ratio in CoFeCMs(CO2) on OFX Degradation

[0040] The different ratios of cobalt and iron in CoFeCMs (CO2) materials affect the activation of the redox cycle of PMS, and thus affect the catalytic degradation performance. This experiment studied the degradation performance of OFX materials synthesized with five ratios of cobalt and iron: 2:1, 1.5:1, 1:1, 1:1.5, and 1:2. Figure 7 As shown, within 0-30 min, the OFX removal rate of CoFeCMs (CO2) with different cobalt and iron ratios reached more than 90%, among which the OFX residual removal rate and removal rate were the best when the cobalt and iron ratio was 1:1.5.

[0041] 2. Effect of calcination temperature on OFX degradation

[0042] This method prepared CoFeCMs(CO2) by two-step calcination. The calcination temperature during the carbonization process affects the specific surface area and pore structure of CoFeCMs(CO2), thereby affecting the catalytic active sites. CoFe@C was prepared at carbonization temperatures of 500℃, 600℃, 700℃, and 800℃, and a series of CoFeCMs(CO2) were synthesized after oxidation in a CO2 atmosphere, such as Figure 8 As shown in the figure, with the increase of carbonization temperature, the removal rate of OFX also gradually increases. When the carbonization temperature is 700℃, the removal rate of OFX by CoFeCMs(CO2) reaches 94.2% within 30min. When the carbonization temperature continues to rise to 800℃, the removal rate of OFX decreases because the carbonization temperature is too high and the structure of CoFeCMs(CO2) is destroyed. Therefore, the optimal carbonization temperature selected in the experiment is 700℃.

[0043] 3. Effects of different catalytic systems on OFX degradation

[0044] The catalytic performance of different systems was investigated, such as Fig. 9As shown in (a), when no PMS is added, the removal rates of OFX by Fe-ZIF 67, CoFeCMs(air) and CoFeCMs(CO2) are very limited, only 19.9%, 7% and 18.2% respectively. When PMS is added, the removal effect of OFX is significantly improved. The removal rates of OFX by Fe-ZIF 67 / PMS, CoFeCMs(air) / PMS and CoFeCMs(CO2) / PMS systems within 30 min are 40.8%, 71.7% and 94.2% respectively. In particular, the removal rate of OFX by CoFeCMs(CO2) / PMS system within 5 min reaches 87.1%, which is significantly higher than that of CoFeCMs(air) / PMS, and the removal rate of OFX within 30 min is also higher than that of CoFeCMs(air) / PMS. Fig. 9 As shown in (b), the reaction kinetic constants of different systems were calculated. The reaction kinetic constant of CoFeCMs(CO2) is 0.526min -1 The reaction kinetic constant of CoFeCMs(air) is 0.0513min -1 This also proves that CoFeCMs(CO2) calcined in a mild CO2 atmosphere have a larger specific surface area and a more complete carbon skeleton, providing more active sites.

[0045] 4. Effect of initial pH on OFX degradation

[0046] The initial pH of the solution will react with the free radicals generated in the catalytic system and the electrons generated on the catalyst surface, thus affecting the degradation efficiency of the catalyst on pollutants to varying degrees. Fig.10 As shown in the figure, at pH = 3, 5, 7, 9, and 11, the degradation efficiency of OFX within 30 min reached 81.2%, 87.3%, 94.2%, 85.1%, and 69.6%, respectively. It is obvious that the CoFeCMs(CO2) / PMS system has a wide pH application range. When the initial pH increases from 7 to 11, the degradation efficiency of OFX decreases significantly, because the hydroxide ions (OH-) convert sulfate radicals (SO4·-) into oxygen radicals (O·-). When the initial pH decreases from 7 to 3, the degradation rate of OFX decreases, because the hydrogen ions (H + ) will remove sulfate radicals and hydroxyl radicals (·OH), which has a certain effect on the degradation of OFX. Based on this, pH = 7 is the optimal initial pH in this experiment.

[0047]

[0048] H + +·OH+e - →H2O (4)

[0049] 5. Effect of PMS addition on OFX degradation

[0050] CoFeCMs(CO2) degrade OFX by activating PMS, such as Fig.11 As shown, when the amount of PMS added is 0.3g / L, 83.7% can be removed within 30 minutes. When the amount of PMS added is increased to 0.5g / L, the removal rate reaches 94.2%. This shows that as the amount of PMS added increases, sufficient doses of PMS can produce more active species such as SO4·- and ·OH, which accelerate and promote the degradation of OFX. However, when the amount of PMS added continues to increase, the removal rate of OFX decreases. When the amount of PMS added is 0.7g / L, the degradation rate of OFX is 86.9%. This is because excessive PMS will cause a quenching reaction, converting SO4·- into SO5 with lower oxidation ability. ·- Therefore, 0.5 g / L is the optimal dosage of PMS in this experiment.

[0051]

[0052]

[0053] 6. Effect of the amount of catalyst CoFeCMs(CO2) added on OFX degradation

[0054] The experiment verified the effect of the amount of catalyst CoFeCMs(CO2) added on the degradation of OFX. Fig.12 As shown, when the addition amount of catalyst CoFeCMs (CO2) is 0.2g / L, 0.3g / L, and 0.4g / L, the removal rate of OFX within 30min is 78.5%, 86.9%, and 94.2%, respectively. With the increase of the addition amount of catalyst CoFeCMs (CO2), the removal rate of OFX also increases accordingly, because the appropriate increase of catalyst CoFeCMs (CO2) provides more active sites. However, when the addition amount of catalyst CoFeCMs (CO2) continues to increase, the removal rate of OFX basically remains at around 92%. Due to the limited content of PMS, there is a situation where it is consumed, which hinders the removal of pollutants. Catalytic degradation effect and operating cost are issues that should be considered in actual application. In this experiment, 0.4g / L is the optimal dosage of catalyst CoFeCMs (CO2).

[0055] 7. Effect of initial OFX concentration on OFX degradation

[0056] The experiment verified the catalytic performance of CoFeCMs(CO2) under different OFX initial concentration conditions. Fig.13As shown in the figure, when the initial concentration of OFX is 10 mg / L, 20 mg / L, and 30 mg / L, the removal rate of OFX is 95.9%, 94.3%, and 89.9% at 30 min. As the initial concentration of OFX increases, the degradation efficiency gradually decreases. This is because the increase in the initial concentration of OFX leads to an increase in the number of OFX molecules in the solution, and the competition between OFX molecules slows down the reaction rate.

[0057] 8. Effect of inorganic anions on OFX degradation

[0058] The experiment verified that four common anions Cl - 、NO3 - 、HCO3 - 、HPO4 2- Effect on the degradation of OFX. Fig.14 As shown, when Cl - When the concentration increased from 0 to 20 mM, the degradation efficiency of OFX decreased from 94.2% to 86.6%, which was due to the fact that Cl - With SO4 ·- , OH reacts to generate Cl · , Cl · The catalytic activity is lower than that of Cl - With SO4 ·- , so the degradation efficiency will be reduced. NO3 - The effect on OFX degradation is similar to that of Cl-. When NO3- concentration increases from 0 to 20mM, the OFX degradation efficiency drops to 77.3%, because NO3- reacts with SO4·- and ·OH to form NO3·. When HCO3- concentration increases, the OFX degradation efficiency is seriously affected. At 20mM, the degradation efficiency drops to 12.9%, because HCO3- reacts with SO4·- and ·OH to form HCO3· and CO3·, whose activity is much lower than SO4·- and ·OH. When HPO4 2 - When the concentration increased to 20 mM, the degradation efficiency of OFX dropped to 83.6% because HPO4 2 - undergoes a quenching reaction with ·OH (Equation 13).

[0059]

[0060] CI - + OH → HCIO · (8)

[0061]

[0062] 9. Effect of actual water on OFX degradation

[0063] In order to further explore the effect of actual water on OFX degradation, OFX solutions were prepared with ultrapure water, Yellow River water and tap water under experimental conditions to explore the effect of different water bodies on OFX degradation. Fig.15 As shown in the figure, the degradation efficiency of OFX solution prepared with ultrapure water, Yellow River water and tap water is 94.2%, 88.1% and 88.1% respectively. The actual water body has a certain influence on the degradation efficiency of OFX, and the degradation rate becomes slow. This may be due to the influence of inorganic anions in the actual water body on the degradation of OFX. But overall, it has excellent removal ability for OFX.

[0064] 10. Cyclic stability analysis of CoFeCMs(CO2) / PMS system

[0065] In practical applications, the stability and reusability of the catalyst are important evaluation indicators of its practicality. Under the same experimental conditions, the catalyst was tested for 5 cycles and XRD characterization was performed on the catalyst after 5 cycles. Fig.16 As shown in (a), after five cycles, the degradation efficiency of OFX reached 85.5%, which still has a high removal efficiency. Fig.16 As shown in (b), the main XRD diffraction peaks of the catalyst after five cycles are basically the same as before degradation, indicating that the crystal structure of the catalyst has not changed during the five degradation processes. And according to the VSM test, CoFeCMs (CO2) has strong magnetism, which makes the catalyst easy to separate in solution. It can be seen that CoFeCMs (CO2) is a catalyst with strong stability, excellent performance, reusability and easy separation.

[0066] 11. Degradation mechanism of MOF-derived CoFeCMs

[0067] (1) Determination of free radicals

[0068] Through free radical quenching experiments, the degradation mechanism of CoFeCMs(CO2) / PMS system on OFX and the types of free radicals that degrade OFX were investigated. Fig.17 As shown in (a), methanol is used as SO4 ·- When 0.2M inhibitor was added, the degradation efficiency of OFX was 79.54% after 30 min, indicating that SO4 ·- When tert-butyl alcohol TBA was used as the quencher of ·OH, after adding 0.2 M TBA, the degradation efficiency of OFX was 90.39% at 30 min, which was slightly lower than the degradation efficiency of 94.2% without TBA, indicating that there was a small amount of ·OH in the reaction system. In addition, furfuryl alcohol FFA and p-benzoquinone p-BQ were used as O2 ·- and 1When the O2 quencher was added to the reaction system, the removal rates of OFX were 24.1% and 60.67%, respectively, indicating that the reaction system had O2 ·- and 1 O2 participates in the reaction and plays a major role.

[0069] To further prove the above speculation, the EPR technique was used to qualitatively analyze the free radical species that degrade OFX. At 1min and 5min, the free radicals were captured using spin traps 5,5-dimethylpyrroline oxide DMPO and 4-oxy-2,2,6,6-tetramethylpiperidine TEMP. Fig.17 As shown in (b), there are four signal peaks with an intensity ratio of 1:2:2:1, which are the signals of DMPO-·OH, and a six-fold signal peak with a peak intensity ratio of 1:1:1:1:1:1, which belongs to DMPO-SO4 ·- . Fig.17 The sextet in (c) corresponds to DMPO-O2 ·- . Fig.17 In (d), three signal peaks with an intensity ratio of 1:1:1 appear, which is TEMP- 1 O2 signal. Based on the above analysis, OH, SO4 ·- 、O2 ·- , 1 Four active components of O2 exist in the process of OFX degradation in CoFeCMs(CO2) / PMS system.

[0070] The electron transfer from OFX to PMS was confirmed by chronoamperometry. Fig.18 As shown in the figure, when CoFeCMs(CO2) was used as the working electrode, the current changed significantly when PMS and OFX were added at 100s and 200s, respectively. The negative current peak appeared at 100s, which was because the added PMS and CoFeCMs(CO2) contacted and significant electron transfer occurred. At 180s, a negative current peak appeared again when OFX was added, indicating that electron transfer occurred between OFX and CoFeCMs(CO2) / PMS.

[0071] (2) Possible degradation pathways of OFX

[0072] In order to explore the possible degradation pathway of OFX by CoFeCMs(CO2) / PMS system, the intermediates in the reaction process were identified by HPLC-MS. According to the analysis results and combined with relevant literature, such as Fig.19As shown, two potential degradation pathways of OFX are described. Pathway one is that the piperazine ring in OFX is completely removed to obtain P1 (m / z=336), and P1 is further decarboxylated and the morpholine ring is removed to obtain P2 (m / z=279) and P3 (m / z=116). The other pathway is that the quinolone part of OFX is decarboxylated and hydroxylated to obtain P4 (m / z=334), and then dealkylated and hydroxylated to generate P5 (m / z=336), and then the piperazine ring of P5 is destroyed to generate the analog P6 (m / z=274), and as the active species oxidize and destroy P6, it is gradually converted into P7 (m / z=175) and P8 (m / z=149). Through a series of reactions, the macromolecular intermediates are converted into small molecular substances, H2O, and CO2.

[0073] (3) Reaction mechanism of OFX degradation by CoFeCMs(CO2) / PMS system

[0074] The degradation mechanism of OFX by CoFeCMs(CO2) / PMS system is as follows Fig. 20 As shown in the figure, CoFe2O4 is evenly distributed on the carbon skeleton of ZIF. The CoFeCMs(CO2) formed by calcination in CO2 atmosphere retains the carbon skeleton as much as possible, which makes CoFeCMs(CO2) have a larger specific surface area and more active sites, making it easier for active substances to transfer and diffuse. The peroxide bond (-OO-) in PMS accepts an electron transferred by Co(Ⅱ) or Fe(Ⅱ) and breaks, and PMS is activated to produce active species. Co(Ⅲ) or Fe(Ⅲ) is reacted with HSO5 - It is reduced to form Co(Ⅱ) or Fe(Ⅱ), forming a complete redox cycle (Formula 14-21). The active species generated (·OH, SO4 ·- 、O2 ·- ,and 1 O2) will oxidize and destroy the structure of OFX, and further mineralize the pollutants into small molecules, H2O, and CO2 (Formula 22).

[0075]

[0076] OH, SO4 ·- , 1 O2+OFX→intermediate product+H2O+CO2(22)

[0077] Compared with the prior art, the present invention has the following beneficial effects:

[0078] In summary, the present invention synthesized dodecahedral Fe-ZIF 67 by coprecipitation, and then synthesized CoFeCMs(CO2) by carbonization and oxidation. Under a mild CO2 atmosphere, the carbon skeleton of Fe-ZIF 67 is less lost during the oxidation process, and the MOF-derived cobalt-iron bimetallic composite CoFeCMs(CO2) prepared by calcination has a larger specific surface area and a complete carbon skeleton, providing more active sites, and has better catalytic performance and electron transfer efficiency. The efficiency of CoFeCMs(CO2) in activating PMS to degrade OFX within 30 minutes can reach 94.2%.

[0079] On the premise of retaining the MOF-derived carbon skeleton, the preparation of MOFs-derived cobalt-iron bimetallic materials can increase the number of active sites and conductivity of the material and improve the catalytic performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] Figure 1 It is the synthesis route of MOF-derived cobalt-iron composite CoFeCMs(CO2);

[0081] Figure 2 Middle: (a) is the SEM image of Fe-ZIF 67;

[0082] (b) is the SEM image of CoFe@C;

[0083] (c) is the SEM image of CoFeCMs(CO2);

[0084] (d) is the SEM image of CoFeCMs(air);

[0085] (e) is the TEM image of CoFeCMs(CO2);

[0086] (f) is the TEM image of CoFeCMs(CO2);

[0087] (g) is the HRTEM image of CoFeCMs(CO2);

[0088] Figure 3 Middle: (a) is the XRD spectra of ZIF 67 and precursor Fe-ZIF 67;

[0089] (b) is the XRD spectra of CoFe@C, CoFeCMs(air), and CoFeCMs(CO2);

[0090] Figure 4 This is the XPS fine spectrum of CoFeCMs(CO2), where: (a) full spectrum; (b) C 1s; (c) O 1s; (d) Fe 2p; (e) Co 2p;

[0091] Figure 5 are the Raman spectra of Fe-ZIF 67, CoFe@C, CoFeCMs(air) and CoFeCMs(CO2);

[0092] Figure 6 (a) is the N2 adsorption-desorption curves of CoFe@C, CoFeCMs(air) and CoFeCMs(CO2); (b) is the pore size distribution;

[0093] Figure 7 The effect of different cobalt-iron ratios on the degradation of OFX. The experimental parameters shown in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, and catalyst concentration is 0.4 g / L;

[0094] Figure 8 It is the effect of calcination temperature on the degradation of OFX. The experimental parameters shown in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, and catalyst concentration is 0.4 g / L;

[0095] Fig. 9 (a) shows the effect of different catalytic systems on the degradation of OFX; (b) shows the reaction rate constants of different catalytic systems. The experimental parameters in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, and catalyst concentration is 0.4 g / L.

[0096] Fig.10 It is the effect of initial pH on the degradation of OFX. The experimental parameters in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, and catalyst concentration is 0.4 g / L;

[0097] Fig.11 It is the effect of PMS addition on the degradation of OFX. The experimental parameters in the figure are: OFX concentration is 20 mg / L, catalyst concentration is 0.4 g / L, pH=7;

[0098] Fig.12 It is the effect of the amount of catalyst added on the degradation of OFX. The experimental parameters in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, pH=7;

[0099] Fig.13 It is the effect of the initial concentration of OFX on the degradation of OFX. The experimental parameters in the figure are: PMS concentration is 0.5 g / L, catalyst concentration is 0.4 g / L, pH = 7;

[0100] Fig.14 The effect of inorganic anions on the degradation of OFX: (a) Cl - , (b) NO3 - , (c) HCO3 -, (d)HPO4 2- , Experimental parameters in the figure: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, catalyst concentration is 0.4 g / L, pH = 7;

[0101] Fig.15 This is the effect of different water bodies on the degradation of OFX. The experimental parameters in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, catalyst concentration is 0.4 g / L, pH = 7;

[0102] Fig.16 (a) is the cyclic stability of the CoFeCMs(CO2) / PMS system. The experimental parameters in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, catalyst concentration is 0.4 g / L, pH=7, (b) is the XRD comparison diagram of CoFeCMs(CO2) before and after the reaction;

[0103] Fig.17 (a) is a free radical quenching experiment, the experimental parameters in the figure are: OFX concentration is 20 mg / L, PMS concentration is 0.5 g / L, catalyst concentration is 0.4 g / L, pH = 7; EPR spectrum of CoFeCMs (CO2) / PMS system: (b) DMPO-·OH and DMPO-SO4 ·- , (c)DMPO-O2 ·- , (d) TEMP- 1 O2;

[0104] Fig.18 is the chronoamperometric curve of CoFeCMs(CO2);

[0105] Fig.19 It is a possible pathway for the degradation of OFX by the CoFeCMs(CO2) / PMS system;

[0106] Fig. 20 This is the reaction mechanism diagram of the CoFeCMs(CO2) / PMS system for the degradation of OFX. DETAILED DESCRIPTION

[0107] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0108] Example 1

[0109] A method for preparing a MOF-derived cobalt-iron composite material comprises the following steps:

[0110] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0111] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0112] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and ultrasonicate them for 10 min as solution B. The molar ratio of Co to Fe in solution B is 1:1.5.

[0113] Under stirring conditions, solution B was slowly added dropwise to solution A, and the mixture was stirred at room temperature for 24 hours. The mixture was centrifuged to collect the solid matter at a speed of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60°C to obtain the precursor Fe-ZIF 67.

[0114] Step 2: Carbonization to prepare CoFe@C:

[0115] The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat, which was then placed in a tube furnace and heated to 700°C at a heating rate of 5°C / min. The mixture was kept in an Ar atmosphere for 2 h to obtain CoFe@C.

[0116] Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2)

[0117] The CoFe@C prepared in step 2 was placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min. A continuous flow of CO2 was introduced into the tubular furnace as a gas atmosphere and kept warm for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

[0118] The MOF-derived cobalt-iron composite was applied to activate peroxymonosulfate to degrade ofloxacin.

[0119] The degradation method is as follows: take 100 mL of OFX solution with a concentration of 20 mg / L and put it into a beaker with a volume of 1000 mL, place the beaker on a shaker and oscillate, add 0.4 g of MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS into the beaker, and use the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to activate PMS to degrade OFX.

[0120] The degradation experiment lasted for 30 minutes. 2-3 mL of the solution in the degradation process was taken out with a syringe, and the solution was filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette. The concentration of OFX was analyzed by UV-Vis spectrophotometry at a wavelength of 294 nm, and the degradation rate of OFX was 94.2%.

[0121] Example 2

[0122] A method for preparing a MOF-derived cobalt-iron composite material comprises the following steps:

[0123] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0124] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0125] Take 0.67mL of 0.8mol / L Co(NO3)2·6H2O and 10.7mL of 0.1mol / L FeCl3·6H2O solution and mix them evenly, dilute them to 12mL with water, and ultrasonicate them for 10min as solution B. The molar ratio of Co to Fe in solution B is 1:2.

[0126] Under stirring conditions, solution B was slowly added dropwise to solution A, and the mixture was stirred at room temperature for 24 hours. The mixture was centrifuged to collect the solid matter at a speed of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60°C to obtain the precursor Fe-ZIF 67.

[0127] Step 2: Carbonization to prepare CoFe@C:

[0128] The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat, which was then placed in a tube furnace and heated to 700°C at a heating rate of 5°C / min. The mixture was kept in an Ar atmosphere for 2 h to obtain CoFe@C.

[0129] Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2)

[0130] The CoFe@C prepared in step 2 was placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min. A continuous flow of CO2 was introduced into the tubular furnace as a gas atmosphere and kept warm for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

[0131] The MOF-derived cobalt-iron composite was applied to activate peroxymonosulfate to degrade ofloxacin.

[0132] The degradation method is as follows: take 100 mL of OFX solution with a concentration of 20 mg / L and put it into a beaker with a volume of 1000 mL, place the beaker on a shaker and oscillate, add 0.4 g of MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS into the beaker, and use the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to activate PMS to degrade OFX.

[0133] The degradation experiment lasted for 30 minutes. 2-3 mL of the solution in the degradation process was taken out with a syringe, and the solution was filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette. The concentration of OFX was analyzed by UV-Vis spectrophotometry at a wavelength of 294 nm, and the degradation rate of OFX was found to be 92.1%.

[0134] Example 3

[0135] A method for preparing a MOF-derived cobalt-iron composite material comprises the following steps:

[0136] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0137] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0138] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and ultrasonicate them for 10 min as solution B. The molar ratio of Co:Fe in solution B is 1:1.5.

[0139] Under stirring conditions, solution B was slowly added dropwise to solution A, and the mixture was stirred at room temperature for 24 hours. The mixture was centrifuged to collect the solid matter at a speed of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60°C to obtain the precursor Fe-ZIF 67.

[0140] Step 2: Carbonization to prepare CoFe@C:

[0141] The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat, which was then placed in a tube furnace and heated to 500°C at a heating rate of 5°C / min. The mixture was kept in an Ar atmosphere for 2 h to obtain CoFe@C.

[0142] Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2)

[0143] The CoFe@C prepared in step 2 was placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min. A continuous flow of CO2 was introduced into the tubular furnace as a gas atmosphere and kept warm for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

[0144] The MOF-derived cobalt-iron composite was applied to activate peroxymonosulfate to degrade ofloxacin.

[0145] The degradation method is as follows: take 100 mL of OFX solution with a concentration of 20 mg / L and put it into a beaker with a volume of 1000 mL, place the beaker on a shaker and oscillate, add 0.4 g of MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS into the beaker, and use the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to activate PMS to degrade OFX.

[0146] The degradation experiment lasted for 30 minutes. 2-3 mL of the solution in the degradation process was taken out with a syringe, and the solution was filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette. The concentration of OFX was analyzed by UV-Vis spectrophotometry at a wavelength of 294 nm, and the degradation rate of OFX was found to be 88.2%.

[0147] Example 4

[0148] A method for preparing a MOF-derived cobalt-iron composite material comprises the following steps:

[0149] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0150] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0151] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and ultrasonicate them for 10 min as solution B. The molar ratio of Co:Fe in solution B is 1:1.5.

[0152] Under stirring conditions, solution B was slowly added dropwise to solution A, and the mixture was stirred at room temperature for 24 hours. The mixture was centrifuged to collect the solid matter at a speed of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60°C to obtain the precursor Fe-ZIF 67.

[0153] Step 2: Carbonization to prepare CoFe@C:

[0154] The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat, which was then placed in a tube furnace and heated to 800°C at a heating rate of 5°C / min. The mixture was kept in an Ar atmosphere for 2 h to obtain carbonized CoFe@C.

[0155] Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2)

[0156] The CoFe@C prepared in step 2 was placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min. A continuous flow of CO2 was introduced into the tubular furnace as a gas atmosphere and kept warm for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

[0157] The MOF-derived cobalt-iron composite was applied to activate peroxymonosulfate to degrade ofloxacin.

[0158] The degradation method is as follows: take 100 mL of OFX solution with a concentration of 20 mg / L and put it into a beaker with a volume of 1000 mL, place the beaker on a shaker and oscillate, add 0.4 g of MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS into the beaker, and use the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to activate PMS to degrade OFX.

[0159] The degradation experiment lasted for 30 minutes. 2-3 mL of the solution in the degradation process was taken out with a syringe, and the solution was filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette. The concentration of OFX was analyzed by UV-Vis spectrophotometry at a wavelength of 294 nm, and the degradation rate of OFX was found to be 68.8%.

[0160] Example 5

[0161] A method for preparing a MOF-derived cobalt-iron composite material comprises the following steps:

[0162] Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method:

[0163] 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A.

[0164] Take 0.8 mL of 0.8 mol / L Co(NO3)2·6H2O and 9.6 mL of 0.1 mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12 mL with water, and ultrasonicate them for 10 min as solution B. The molar ratio of Co to Fe in solution B is 1:1.5.

[0165] Under stirring conditions, solution B was slowly added dropwise to solution A, and the mixture was stirred at room temperature for 24 hours. The mixture was centrifuged to collect the solid matter at a speed of 8000 rpm. The solid matter was then repeatedly washed with water and methanol alternately for several times and dried at 60°C to obtain the precursor Fe-ZIF 67.

[0166] Step 2: Carbonization to prepare CoFe@C:

[0167] The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat, which was then placed in a tube furnace and heated to 700°C at a heating rate of 5°C / min. The mixture was kept in an Ar atmosphere for 2 h to obtain CoFe@C.

[0168] Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2)

[0169] The CoFe@C prepared in step 2 was placed in a tubular furnace and heated to 500°C at a heating rate of 5°C / min. A continuous flow of CO2 was introduced into the tubular furnace as a gas atmosphere and kept warm for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

[0170] The MOF-derived cobalt-iron composite was applied to activate peroxymonosulfate to degrade ofloxacin.

[0171] The degradation method is as follows: take 100 mL of OFX solution with a concentration of 20 mg / L and put it into a beaker with a volume of 1000 mL, place the beaker on a shaker and oscillate, add 0.6 g of MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS into the beaker, and use the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to activate PMS to degrade OFX.

[0172] The degradation experiment lasted for 30 minutes. 2-3 mL of the solution in the degradation process was taken out with a syringe, and the solution was filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette. The concentration of OFX was analyzed by UV-Vis spectrophotometry at a wavelength of 294 nm, and the degradation rate of OFX was found to be 91.1%.

[0173] Example 6

[0174] The MOF-derived cobalt-iron composite material CoFeCMs (CO2) prepared in Example 1 was applied to the degradation of ofloxacin. The degradation method was the same as in Example 1. The degradation time was 30 min each time and the process was repeated 5 times. After each degradation of the pollutant, the CoFeCMs (CO2) catalyst was recovered and the recovered CoFeCMs (CO2) catalyst was washed with deionized water. The CoFeCMs (CO2) catalyst was repeatedly used and the concentration of OFX in the pollutant after each degradation was analyzed. The degradation rate of OFX after the fifth cycle was 85.5%.

[0175] The above are only preferred embodiments of the present invention. It should be noted that for those skilled in the art, under the technical enlightenment provided by the present invention, other equivalent variations and improvements can also be made, which should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a MOF-derived cobalt-iron composite material, characterized in that: The following steps are involved: Step 1: Prepare the precursor Fe-ZIF 67 by co-precipitation method: 10 mL of 1 mol / L NaOH and 10 mL of 3.36 mol / L 2-methylimidazole solution were mixed and stirred evenly, and the mixture was ultrasonicated for 10 min. The prepared solution was referred to as solution A. Take 0.67-0.8mL of 0.8mol / L Co(NO3)2·6H2O and 9.6-10.7mL of 0.1mol / L FeCl3·6H2O solution, mix them evenly, dilute them to 12mL with water, and use them as solution B after ultrasonic treatment for 10min. The molar ratio of Co element to Fe element in solution B is 1:1.5-2; Solution B was slowly added dropwise to solution A under stirring. After the addition was completed, stirring was continued at room temperature for 24 h. The mixture was centrifuged to collect the solids. The solids were then repeatedly washed with water and methanol alternately for several times and dried at 60 °C to obtain the precursor Fe-ZIF 67. Step 2: Carbonization to prepare CoFe@C: The precursor Fe-ZIF 67 prepared in step 1 was ground into powder and placed in a porcelain boat in a tube furnace, heated to 500-800°C, and kept warm for 2 hours under Ar atmosphere to obtain CoFe@C; Step 3: Calcination under CO2 atmosphere to synthesize MOF-derived cobalt-iron composite material CoFeCMs(CO2): The CoFe@C prepared in step 2 is placed in a tubular furnace, the temperature is raised to 500°C, a continuous flow of CO2 is introduced into the tubular furnace as a gas atmosphere, and the temperature is kept for 1 hour to obtain a MOF-derived cobalt-iron composite material CoFeCMs(CO2).

2. The method for preparing a MOF-derived cobalt-iron composite material according to claim 1, characterized in that: The heating rate of the tubular furnace in step 2 is 5°C / min.

3. The method for preparing a MOF-derived cobalt-iron composite material according to claim 1, characterized in that: The heating rate of the tubular furnace in step 3 is 5°C / min.

4. The method for preparing a MOF-derived cobalt-iron composite material according to claim 1, characterized in that: The centrifugal speed of the mixed solution in step 1 is 8000 rpm.

5. An application of a MOF-derived cobalt-iron composite material, characterized in that: The MOF-derived cobalt-iron composite was applied to activate peroxymonosulfate to degrade ofloxacin.

6. The use of the MOF-derived cobalt-iron composite material according to claim 5, characterized in that: The degradation method is as follows: 100 mL of OFX solution with a concentration of 20 mg / L is put into a 1000 mL beaker, the beaker is placed on a shaker for shaking, 0.4-0.6 g of a MOF-derived cobalt-iron composite material CoFeCMs(CO2) and 0.5 g of PMS are added to the beaker, and the PMS is activated by the synergistic effect of the cobalt-iron bimetallic in the MOF-derived cobalt-iron composite material CoFeCMs(CO2) to degrade OFX; The degradation time was 30 min. 2-3 mL of the solution in the degradation process was taken out with a syringe. The solution was filtered with a 0.22 μm polyethersulfone PES filter membrane and placed in a quartz cuvette. The OFX concentration was analyzed with UV-Vis at a wavelength of 294 nm. The degradation rate of OFX was 68.8-94.2%.

Citation Information

Patent Citations

  • MOF-74-based cobalt-iron bimetallic catalytic material as well as preparation method and application thereof

    CN110075922A

  • Hollow magnetic composite carbon material derived based on metal-organic framework material, derivation method thereof, and wastewater treatment method

    CN113522290A

  • Preparation of biochar-modified ferrocobalt bimetallic composite catalyst and application of biochar-modified ferrocobalt bimetallic composite catalyst in catalytic degradation of tetracycline

    CN114425340A

  • Method for degrading ciprofloxacin by efficiently activating peroxymonosulfate

    CN116924552A

  • Ferrocobalt MOF-derived nanocube material as well as preparation method and application thereof