Catalyst for preparing difluoromethane or monochlorodifluoromethane as well as preparation method and application of catalyst

By using antimony oxide combined with metal sulfate or phosphate and support catalysts to replace traditional antimony chloride catalysts, the problems of easy deactivation of antimony chloride catalysts and equipment corrosion are solved, and high-efficiency and low-cost difluoromethane are achieved and difluorommonochloromethane production extends the life of the equipment and improves product purity and conversion.

CN118988351APending Publication Date: 2024-11-22LINHAI LIMIN CHEM

Patent Information

Application Number
CN202411077938.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The antimony chloride catalyst used in the existing production processes of difluoromethane and difluorommonochloromethane are prone to deactivation, resulting in serious equipment corrosion and by-product generation, and the process conditions are harsh, affecting production efficiency and product purity.

Method used

Using antimony oxide and metal aluminum, zinc, iron sulfate or phosphate as cocatalysts, combined with activated carbon, alumina or magnesium oxide as support, as catalysts, and replaces the traditional production method and process flow through improved preparation methods and process flow. Antimony chloride catalyst, improves the activity and service life of the catalyst.

Benefits of technology

It realizes long-term and stable use of the catalyst without inactivation, reduces equipment corrosion, improves the purity and conversion of difluoromethane and difluorommonochloromethane, extends the service life of the reaction equipment, and reduces three waste pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing difluoromethane or monochlorodifluoromethane and a preparation method and application thereof.The catalyst is formed by mixing antimony oxide and a cocatalyst, and the cocatalyst comprises sulfate or phosphate of metal aluminum, zinc and iron and a carrier, the carrier is one or a mixture of more than two of activated carbon, aluminum oxide and magnesium oxide. The catalyst disclosed by the invention is low in cost, easy in technical operation, less in three wastes, convenient in post-treatment and small in corrosion to equipment, and also has the advantages of high activity, long-term use and no deactivation phenomenon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a catalyst and a preparation method and application thereof, in particular to a catalyst for preparing difluoromethane or difluorochloromethane and a preparation method and application thereof. Background Art

[0002] Difluoromethane is a good refrigerant and an important intermediate for fluorinated drugs. The chemical formula of difluoromethane (HFC-32) is CH2F2, the potential for depleting the atmospheric ozone layer (ODP) is 0, the global warming potential (GWP) is 0.12, and it has excellent environmental performance and performance. The mixture with other ODS substitutes such as pentafluoroethane (HFC-125) is used as a refrigerant to replace difluorochloromethane (HCFC-22), and it occupies an important position in ODS substitutes, and its development prospects are very broad.

[0003] Chlorodifluoromethane (HCFC-22, R22), also known as Freon-22, is a colorless, nearly odorless gas at room temperature. It has the advantages of being non-combustible, non-corrosive, extremely low in toxicity, and having good chemical and thermal stability. It is insoluble in water but soluble in ethanol. It is often used as a solvent, aerosol propellant, and a high-performance HCFC-type medium and low-temperature refrigerant. It can also be used as a chemical raw material for the production of tetrafluoroethylene and its downstream products, and the production of new refrigerants for ODS substitutes and new fluorine-containing polymer materials.

[0004] The production process of difluoromethane is mainly to use dichloromethane and HF or KF for fluorination reaction. In the laboratory, it can sometimes be produced by catalytic hydrogenation dechlorination of hydrochlorofluorocarbons and fluorination at 200-280°C using formaldehyde and HF with chromium or its fluoride oxide as catalyst. In production, difluoromethane is prepared by using dichloromethane and HF, and antimony chloride is used as a catalyst for fluorination. The production process of difluoromonochloromethane is also mainly to use trichloromethane and hydrogen fluoride for substitution reaction under the catalysis of antimony pentachloride. The preparation of fluorocarbon compounds by fluorination of chloroalkanes is mainly liquid phase fluorination and gas phase fluorination. When using antimony pentachloride catalyst in liquid phase fluorination, catalyst additives need to be added, the process conditions are harsh, the equipment is severely corroded, and a large amount of three wastes are generated. The gas phase fluorination method has less pollution of three wastes and can be produced continuously, but it is very easy to produce a series of by-products such as dichloromonofluoromethane and trifluoromethane in the process of generating difluoromonochloromethane. Moreover, in the production of difluoromethane and difluorochloromethane, antimony chloride series compounds are required as catalysts. This series of catalysts are easily deactivated during the catalytic process and are difficult to handle. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a catalyst for preparing difluoromethane or difluoromonochloromethane, a preparation method of the catalyst and the application of the catalyst in the production of difluoromethane or difluoromonochloromethane. The catalyst has high activity and has no deactivation phenomenon after long-term use.

[0006] In order to solve the above technical problems, the present invention first discloses a catalyst for preparing difluoromethane or difluoromonochloromethane, wherein the catalyst is a mixture of antimony oxide and a promoter, wherein the promoter includes a sulfate or phosphate of metal aluminum, zinc, or iron and a carrier, and the carrier is one or a mixture of two or more of activated carbon, aluminum oxide, or magnesium oxide in any ratio.

[0007] Furthermore, the antimony oxide is one of antimony trioxide, antimony pentoxide, antimony tetroxide, or a mixture of two or more of them in any ratio.

[0008] Furthermore, the sulfate or phosphate of metal aluminum, zinc or iron is one or a mixture of any ratio of two or more of Al2(SO4)3, ZnSO4, Fe2(SO4)3, AlPO4, Fe3(PO4)2, Zn3(PO4)2.

[0009] Furthermore, the mass percentage of the promoter and antimony oxide in the catalyst is 80-90:10-20.

[0010] Furthermore, the mass percentage of the carrier and the sulfate or phosphate of metal aluminum, zinc, and iron in the co-catalyst is 80-90:10-20.

[0011] The present invention also discloses a method for preparing the above catalyst, which comprises the following steps:

[0012] (1) Mix the carrier and a saturated solution of a sulfate or phosphate of metal aluminum, zinc or iron in deionized water, filter to obtain a filter cake, let the filter cake stand to dry, dry it thoroughly in a dryer at 200-250° C., grind it into powder with a grinder, and pass it through a 200-300 mesh sieve to obtain a co-catalyst;

[0013] (2) Mixing the promoter with antimony oxide to obtain a catalyst.

[0014] Furthermore, in step (1), the carrier is first subjected to a vacuum treatment at a pressure of -0.3 to -0.6 MPa, generally for about 15 minutes, to remove fine particles in the carrier.

[0015] Furthermore, in step (2), in order to facilitate the loading of the catalyst, the co-catalyst and antimony oxide are first mixed with dichloromethane or chloroform and then pressed into the reactor for mixing.

[0016] The present invention also discloses an application of the above catalyst or the catalyst prepared by the above method in the preparation of difluoromethane or difluoromonochloromethane. The raw materials dichloromethane or trichloromethane and hydrogen fluoride are introduced into a preheater for preheating, and then introduced into a reactor containing the catalyst. The temperature is 80-150°C and the reaction pressure is 1-18 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the materials enter the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for application; difluoromethane or difluoromonochloromethane and hydrogen chloride are separated at the top, and hydrogen chloride and other acidic gases are removed by water washing and alkali washing or dry separation to obtain difluoromethane or difluoromonochloromethane crude products, which are then purified twice to obtain the product.

[0017] The fluorination catalyst of the present invention replaces antimony chloride with antimony oxide, and the co-catalyst is composed of sulfate or phosphate of metal aluminum, zinc, and iron and a carrier. The catalyst formula design is novel, the technical route is advanced, and it has certain originality. The preparation process is simple, the cost is low, and it is easy to operate. There is no three wastes, and the corrosion to the equipment is small. The service life of the reaction equipment for producing difluoromethane is extended from 6 months to more than 12-18 months; the service life of the reaction equipment for producing difluoromonochloromethane is extended from 12-18 months to more than 24-36 months. The catalyst of the present invention has high activity, can be used for a long time, and there is no deactivation phenomenon in continuous production (at least one year or more). The catalyst is used to prepare difluoromethane or difluoromonochloromethane, the process is simple, and the purity of the obtained difluoromethane or difluoromonochloromethane is as high as more than 99.9%, and the conversion rate is as high as more than 94%. DETAILED DESCRIPTION

[0018] The present invention is further explained below in conjunction with the examples. The following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0019] Example 1

[0020] Preparation of activated carbon supported co-catalyst

[0021] A certain amount of activated carbon was vacuumed for 15 minutes under a -0.3Mpa vacuum pump, and 80kg of the activated carbon after vacuuming was weighed. In addition, 20kg of aluminum sulfate was prepared into a saturated solution with deionized water at room temperature and pressure. Then, the activated carbon and the saturated aluminum sulfate solution were fully mixed and stirred, and the filter cake was filtered to obtain a filter cake, and the filter cake was placed to dry, and the dried filter cake was placed in a 200℃ dryer to be thoroughly dried and dehydrated, and ground into powder by a grinder, and sieved through 200 mesh to obtain a catalyst promoter 1.

[0022] Fluorination catalyst prepared from the co-catalyst 1

[0023] 90 kg of the powder of the promoter 1 was mixed with 200 kg of dichloromethane and then pressed into the reactor. Then, 10 kg of antimony trioxide was mixed with 20 kg of dichloromethane and then pressed into the reactor. The mixture was further mixed to obtain the fluorination catalyst 1.

[0024] Application of fluorination catalyst 1 in the preparation of difluoromethane

[0025] In a reactor already loaded with fluorination catalyst 1, 141 kg / h of dichloromethane and 67 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to 30°C and then pressed into the reactor. The reaction temperature was 150°C and the reaction pressure was 18 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material enters the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromethane. After secondary drying and water removal, the product is 85.0kg / h, with a conversion rate of 98.5% and a purity of 99.9%.

[0026] Application of fluorination catalyst 1 in the preparation of difluorochloromethane

[0027] The dichloromethane used for mixing with the promoter 1 and antimony trioxide in the fluorination catalyst 1 was replaced with chloroform.

[0028] In a reactor equipped with fluorination catalyst 1, 200 kg / h of chloroform and 71 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to about 30°C and then pressed into the reactor. The reaction temperature was 80°C and the reaction pressure was 10 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material is distilled into a condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromonochloromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromonochloromethane. After secondary drying and water removal, the product is 137.2kg / h, with a conversion rate of 95% and a purity of 99.9%.

[0029] Example 2

[0030] Preparation of alumina supported co-catalyst

[0031] A certain amount of aluminum oxide was vacuumed for 15 minutes under a -0.3Mpa vacuum pump, and 90kg of the aluminum oxide after vacuuming was weighed. In addition, 10kg of ferric sulfate was prepared into a saturated solution with ionized water at room temperature and pressure. Then, the aluminum oxide and the saturated solution of ferric sulfate were fully mixed and stirred, and the filter cake was obtained by suction filtration. The filter cake was left to stand and dry, and the dried filter cake was placed in a 250°C drying machine for thorough drying and dehydration, and ground into powder by a grinder, and sieved through 200 mesh to obtain the catalyst promoter 2.

[0032] Fluorination catalyst prepared from cocatalyst 2

[0033] 90 kg of the co-catalyst 2 powder was mixed with 200 kg of dichloromethane and then pressed into the reactor. Then 8 kg of antimony trioxide, 2 kg of antimony pentoxide and 20 kg of dichloromethane were mixed and then pressed into the reactor. The mixture was further mixed to obtain the fluorination catalyst 2.

[0034] Application of fluorination catalyst 2 in the preparation of difluoromethane

[0035] In a reactor equipped with fluorination catalyst 2, 130 kg / h of dichloromethane and 65 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to about 30°C and then pressed into the reactor. The reaction temperature was 50°C and the reaction pressure was 5 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material enters the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromethane. After secondary drying and water removal, the product is 76.5kg / h, with a conversion rate of 96.2% and a purity of 99.9%.

[0036] Application of fluorination catalyst 2 in the preparation of difluorochloromethane

[0037] The dichloromethane used for mixing with the promoter 2, antimony trioxide and antimony pentoxide in the fluorination catalyst 2 was replaced with chloroform.

[0038] In a reactor equipped with a fluorination catalyst, 221 kg / h of chloroform and 79 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to about 30°C and then pressed into the reactor. The reaction temperature was 100°C and the reaction pressure was 10 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material enters the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromonochloromethane and hydrogen chloride are separated at the top and acid gases such as hydrogen chloride are removed by water and alkali washing to obtain crude difluoromonochloromethane. After secondary drying and water removal, the product is 150.4kg / h, with a conversion rate of 94% and a purity of 99.9%.

[0039] Example 3

[0040] Preparation of magnesium oxide supported co-catalyst

[0041] A certain amount of magnesium oxide was vacuumed for 15 minutes under a -0.3Mpa vacuum pump, and 90kg of magnesium oxide after vacuuming was weighed. In addition, 10kg of zinc sulfate was prepared into a saturated solution with deionized water at normal temperature and pressure. Then, the vacuumed magnesium oxide and the saturated zinc sulfate solution were fully mixed and stirred, and filtered to obtain a filter cake, and the filter cake was left to stand and dry, and the dried filter cake was placed in a 220°C drying machine for thorough drying and dehydration, ground into powder by a grinder, and sieved through 200 mesh to obtain a co-catalyst 3.

[0042] Fluorination catalyst prepared from cocatalyst 3

[0043] 90 kg of the co-catalyst 3 powder was mixed with 200 kg of dichloromethane and then pressed into the reactor. Then 5 kg of antimony pentoxide and 5 kg of antimony tetroxide were mixed with 20 kg of dichloromethane and then pressed into the reactor. The mixture was further mixed to obtain the fluorination catalyst 3.

[0044] Application of fluorination catalyst 3 in the preparation of difluoromethane

[0045] In a reactor equipped with fluorination catalyst 3, 125 kg / h of dichloromethane and 60 kg / h of hydrogen fluoride were preheated in a preheater and pressed into the reactor. At a temperature of 100°C and a pressure of 10 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material is distilled into a condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromethane. After secondary drying and water removal, the product is 73.4kg / h, with a conversion rate of 96% and a purity of 99.9%.

[0046] Example 4

[0047] Preparation of magnesium oxide / activated carbon supported co-catalyst

[0048] A certain amount of magnesium oxide and activated carbon were vacuumed for 15 minutes under a -0.3Mpa vacuum pump, and 50kg of magnesium oxide and 40kg of activated carbon after vacuuming were weighed. In addition, 10kg of ferric sulfate was prepared into a saturated solution with deionized water at room temperature and pressure. Then, magnesium oxide, activated carbon and saturated ferric sulfate solution were fully mixed and stirred, and filtered to obtain a filter cake, and the filter cake was left to stand and dry, and the dried filter cake was placed in a 220°C drying machine for thorough drying and dehydration, and ground into powder by a grinder, and sieved through 300 mesh to obtain a catalyst promoter 4.

[0049] Fluorination catalyst prepared from cocatalyst 4

[0050] 90 kg of the co-catalyst 4 powder was mixed with 200 kg of chloroform and then pressed into the reactor. Then, 10 kg of antimony trioxide was mixed with 20 kg of chloroform and then pressed into the reactor. The mixture was further mixed to obtain the fluorination catalyst 4.

[0051] Application of fluorination catalyst 4 in the preparation of difluorochloromethane

[0052] In a reactor equipped with fluorination catalyst 4, 200 kg / h of chloroform and 71 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to about 30°C and then pressed into the reactor. The reaction temperature was 120°C and the reaction pressure was 8 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material enters the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromonochloromethane and hydrogen chloride are separated at the top and acid gases such as hydrogen chloride are removed by water and alkali washing to obtain crude difluoromonochloromethane. After secondary drying and water removal, the product is 137.5kg / h, with a conversion rate of 95% and a purity of 99.99%.

[0053] Example 5

[0054] Preparation of magnesium oxide / aluminum oxide supported co-catalyst

[0055] Magnesium oxide and aluminum oxide were vacuumed for 15 minutes under a vacuum pump of -0.5Mpa, and then 40kg of magnesium oxide and 40kg of aluminum oxide that had been vacuumed were weighed. In addition, 10kg of zinc sulfate and 10kg of ferric sulfate were prepared into a saturated solution with deionized water at normal temperature and pressure. Then, magnesium oxide, aluminum oxide and the saturated solution of zinc sulfate and ferric sulfate were fully mixed and stirred, and filtered to obtain a filter cake, and the filter cake was left to stand and dry, and the dried filter cake was placed in a 220°C drying machine to be thoroughly dried and dehydrated, and ground into powder by a grinder, and sieved through 300 mesh to obtain a co-catalyst 5.

[0056] Fluorination catalyst prepared from cocatalyst 5

[0057] 90 kg of the co-catalyst 5 powder was mixed with 200 kg of dichloromethane and pressed into the reactor. Then, 8 kg of antimony trioxide, 2 kg of antimony pentoxide and 20 kg of dichloromethane were mixed and pressed into the reactor, and then further mixed to obtain the fluorination catalyst 5.

[0058] Application of fluorination catalyst 5 in the preparation of difluoromethane

[0059] In a reactor equipped with fluorination catalyst 5, 141 kg / h of dichloromethane and 67 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to 30°C and then pressed into the reactor. The reaction temperature was 150°C and the reaction pressure was 18 kg / cm 2The reaction is carried out under absolute pressure. After the reaction is completed, the materials enter the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromethane. After secondary drying and water removal, the product is 85kg / h, with a conversion rate of 98.5% and a purity of 99.9%.

[0060] Example 6

[0061] Preparation of magnesium oxide / aluminum oxide / activated carbon supported co-catalyst

[0062] Magnesium oxide, aluminum oxide and activated carbon were vacuumed for 15 minutes under a vacuum pump of -0.4Mpa, and 30kg of magnesium oxide, 30kg of aluminum oxide and 30kg of activated carbon after vacuum treatment were weighed. In addition, 10kg of aluminum phosphate and 10kg of ferric sulfate were prepared into a saturated solution with deionized water at room temperature and pressure. Then, magnesium oxide, aluminum oxide, activated carbon and the saturated solution of aluminum phosphate and ferric sulfate were fully mixed and stirred, and filtered to obtain a filter cake, and the filter cake was left to stand and dry, and the dried filter cake was placed in a 220℃ drying machine for thorough drying and dehydration, ground into powder by a grinder, and sieved through 300 mesh to obtain a catalyst promoter 6.

[0063] Fluorination catalyst prepared from cocatalyst 6

[0064] 90 kg of the co-catalyst 6 powder was mixed with 200 kg of dichloromethane and pressed into the reactor. Then, 5 kg of antimony pentoxide and 5 kg of antimony tetroxide were mixed with 20 kg of dichloromethane and pressed into the reactor. The mixture was further mixed to obtain the fluorination catalyst 6.

[0065] Application of fluorination catalyst 6 in the preparation of difluoromethane

[0066] In a reactor equipped with fluorination catalyst 6, 141 kg / h of dichloromethane and 67 kg / h of hydrogen fluoride were preheated to 30°C in a preheater and then pressed into the reactor. The reaction temperature was 150°C and the reaction pressure was 18 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the materials enter the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromethane. After secondary drying and water removal, the product is 85kg / h, with a conversion rate of 98.5% and a purity of 99.9%.

[0067] Application of fluorination catalyst 6 in the preparation of difluorochloromethane

[0068] The dichloromethane mixed with the promoter 6, antimony pentoxide and antimony tetroxide in the fluorination catalyst 6 is replaced with chloroform.

[0069] In a reactor equipped with fluorination catalyst 6, 200 kg / h of chloroform and 71 kg / h of hydrogen fluoride were respectively introduced into a preheater to be preheated to about 30°C and then pressed into the reactor. The reaction temperature was 120°C and the reaction pressure was 8 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the material enters the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for recycling. Difluoromonochloromethane and hydrogen chloride are separated at the top and washed with water and alkali to remove acidic gases such as hydrogen chloride to obtain crude difluoromonochloromethane. After secondary drying and water removal, the product is 139kg / h, with a conversion rate of 96% and a purity of 99.99%.

Claims

1. A catalyst for preparing difluoromethane or difluorochloromethane, characterized in that: The catalyst is formed by mixing antimony oxide and a promoter, wherein the promoter includes sulfate or phosphate of metal aluminum, zinc, iron and a carrier, and the carrier is one or a mixture of two or more of activated carbon, aluminum oxide and magnesium oxide.

2. The catalyst according to claim 1, characterized in that: The antimony oxide is one of antimony trioxide, antimony pentoxide, antimony tetroxide, or a mixture of two or more thereof.

3. The catalyst according to claim 1, characterized in that: The sulfate or phosphate of metal aluminum, zinc or iron is one or a mixture of two or more of Al2(SO4)3, ZnSO4, Fe2(SO4)3, AlPO4, Fe3(PO4)2, Zn3(PO4)2.

4. The catalyst according to claim 1, characterized in that: The mass percentage of the promoter and the antimony oxide in the catalyst is 80-90:10-20.

5. The catalyst according to claim 1, characterized in that: The mass percentage of the carrier and the sulfate or phosphate of metal aluminum, zinc and iron in the co-catalyst is 80-90:10-20.

6. A method for preparing a catalyst according to any one of claims 1 to 5, characterized in that The preparation method comprises the following steps: (1) Mix the carrier and a saturated solution of a sulfate or phosphate of metal aluminum, zinc or iron uniformly, filter to obtain a filter cake, let the filter cake stand to dry, dry it thoroughly in a dryer at 200-250° C., grind it into powder with a grinder, and pass it through a 200-300 mesh sieve to obtain a co-catalyst; (2) Mixing the promoter with antimony oxide to obtain a catalyst.

7. The preparation method according to claim 6, characterized in that: In step (1), the carrier is first subjected to vacuum treatment at a pressure of -0.3 to -0.6 MPa.

8. The preparation method according to claim 6, characterized in that: In step (2), the promoter and antimony oxide are first mixed with dichloromethane or chloroform, and then pressed into the reactor for mixing.

9. Use of the catalyst according to any one of claims 1 to 5 or the catalyst prepared by the method according to any one of claims 6 to 8 in the preparation of difluoromethane or difluorochloromethane, characterized in that: The raw materials of dichloromethane or chloroform and hydrogen fluoride are passed into a preheater for preheating, and then passed into a reactor containing a catalyst, the temperature is 80-150°C, the reaction pressure is 1-18 kg / cm 2 The reaction is carried out under absolute pressure. After the reaction is completed, the materials enter the condensation separation tower for separation. The by-products separated at the bottom of the separation tower are recycled to the reactor for application; difluoromethane or difluoromonochloromethane and hydrogen chloride are separated at the top, and hydrogen chloride and other acidic gases are removed by water washing and alkali washing or dry separation to obtain difluoromethane or difluoromonochloromethane crude products, which are then purified twice to obtain the product.

Citation Information

Patent Citations

  • Fluorination catalyst for preparing difluoromethane or monochlorodifluoromethane, preparation method and application

    CN102527414A

  • Method for producing difluoromethane

    CN104703954A

  • Preparation method of 1,1,1-trifluoroethane

    CN109809960A

  • Process and system for stable production of difluoromethane

    CN113698270A

  • Process for producing 1,3,3,3-tetrafluoropropene

    JP2010100613A

Cited By

  • Monolithic catalyst for hydrogen production through ammonia decomposition as well as preparation method and application of monolithic catalyst

    CN121513905A