Nitrogen-defect metal-free flower-cluster-shaped C3N4 photocatalyst, preparation method and application in degradation of tetracycline antibiotics

Through the preparation of nitrogen-deficient metal-free flower cluster C3N4 photocatalyst, the problems of low antibiotic pollution treatment efficiency and semiconductor photocatalysts in the prior art are solved, and efficient and low-cost removal of tetracycline antibiotics are achieved, and the catalyst can be reused. , environmentally friendly.

CN118988367APending Publication Date: 2024-11-22JIASHAN ADIMAN WATER TECH

Patent Information

Application Number
CN202410970375.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When dealing with antibiotic pollution, especially tetracycline hydrochloride, the removal efficiency is not ideal, the cost is high, and the secondary pollution problem exists. The commonly used semiconductor photocatalysts have problems such as expensive raw materials, high toxicity, low efficiency, and unstable activity. Limits its practical application.

Method used

The C3N4 photocatalyst with nitrogen-deficient metal flower-free clusters was prepared by a single urea as the precursor, which improved the specific surface area and photocatalytic performance, and was used to efficiently remove tetracycline antibiotics.

Benefits of technology

The degradation rate of tetracycline antibiotics is achieved efficiently to achieve more than 98%, simple operation, low cost, reusable catalyst, and free of metals, and environmentally friendly, solving the problems of low removal efficiency and secondary pollution in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988367A_ABST
    Figure CN118988367A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of photocatalytic materials, and provides a nitrogen-defect metal-free flower-cluster-shaped C3N4 photocatalyst, a preparation method and application in degradation of tetracycline antibiotics. Single urea is used as a precursor, and the metal-free flower-shaped C3N4 photocatalyst is prepared through a thermal polymerization reaction at 500-600 DEG C. The operation process is simple, the raw materials are economical and cheap, the obtained catalyst is stable in performance and good in catalytic effect, and the problem that large-scale production cannot be achieved due to limitation of the process and the raw materials in an existing C3N4 preparation method is solved. The prepared C3N4 shows excellent photocatalytic activity on degradation of the tetracycline antibiotics, more than 85% of the tetracycline antibiotics are still removed after the C3N4 is repeatedly used for 4 times, and it is indicated that the material has good repeatability and stability. The novel photocatalyst prepared by the invention and establishment of an effective tetracycline antibiotic degradation method provide a new thought.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic materials, and in particular relates to a nitrogen-deficient metal-free flower cluster-shaped C3N4 photocatalyst, a preparation method thereof, and an application in degrading tetracycline antibiotics. Background Art

[0002] In the past few decades, with the rapid development of urbanization and industrialization, antibiotics have been widely used in the fields of medicine and animal husbandry. As a new type of refractory organic pollutant, antibiotic pollution has become a global problem. Due to its wide distribution in the environment, high concentration and strong drug resistance, it seriously threatens the natural ecological environment and human health and safety. Among many antibiotics, tetracycline hydrochloride (TCH), as the second largest broad-spectrum antibiotic in the world, is widely used in aquaculture and animal husbandry. However, the effective absorption rate of TCH by livestock is less than 30%. Under normal circumstances, residual TCH is easily accumulated in aquatic systems, which not only causes fatal genotoxicity and neurotoxicity in biological systems, but also is mostly discharged into the environment with feces and urine, seriously polluting soil and water bodies. Therefore, it is urgent to seek a simple and efficient measure to eliminate TCH in wastewater. At present, various technologies such as physical adsorption, biodegradation and chemical advanced oxidation have been applied to solve this problem. However, due to the stable chemical structure and poor biodegradability of TCH, the above methods have disadvantages such as unsatisfactory removal efficiency, high cost or secondary pollution when treating TCH, and it is difficult to achieve satisfactory results.

[0003] In recent years, sunlight-powered semiconductor photocatalysis technology has been considered as the most promising strategy for eliminating refractory organic pollutants due to its unique advantages of simple operation, eco-friendliness, strong photooxidation ability, and high mineralization rate. To date, various semiconductor materials have been developed and further used as photocatalysts, including TiO2, ZnO, WO3, black phosphorus, BiOBr, etc. However, most semiconductor-mediated photocatalysis has problems such as expensive raw materials, high toxicity, low efficiency, and unstable activity, which increases the technical threshold for the practical application of photocatalysis. Therefore, the preparation of efficient, low-cost, metal-free photocatalysts is of great significance and is also a necessary prerequisite for efficient photodegradation.

[0004] Carbon nitride (C3N4) is a metal-free semiconductor with a melon-seed structure. It has attracted great interest from scientists due to its suitable band gap (2.7 eV), tunable electronic properties, good chemical stability, and better economic and environmental effects. Recently, C3N4 has been regarded as one of the most promising technologies for clean energy development and environmental pollution remediation, while facing the long-term challenge of achieving broad light absorption and high specific surface area, especially high charge transfer. However, the narrow utilization of visible light, low specific surface area, and low migration efficiency of photogenerated electrons and holes limit the development of C3N4. Therefore, many effective methods have been proposed to promote the photocatalytic efficiency of g-C3N4, including constructing heterojunctions, designing structures, depositing precious metals, etc. Among them, morphology control can simultaneously increase the specific surface area (surface active sites), accelerate charge separation, and improve the light absorption range, thus becoming one of the most important research strategies. Therefore, in order to improve the catalytic efficiency of C3N4, modifying C3N4 by controlling the morphology is a very effective way. Summary of the invention

[0005] The purpose of the present invention is to provide a nitrogen-deficient metal-free flower cluster C3N4 photocatalyst and a preparation method thereof and application in the degradation of tetracycline antibiotics.

[0006] The present invention is realized by the following technical scheme: a nitrogen-deficient metal-free flower-like C3N4 photocatalyst is prepared by using single urea as a precursor through a thermal polymerization reaction at 500-600°C for 2-4h.

[0007] The method for preparing the nitrogen-deficient metal-free flower cluster-shaped C3N4 photocatalyst is specifically as follows: 1) 8-12g urea was added with 10ml secondary water, stirred thoroughly, and ultrasonicated for 5min to obtain a clear solution; the clear solution was dried at 100℃ for 6h, and then heated to 500-600℃ at a heating rate of 10℃ / min and continued to react for 2-4h to obtain a CDs@C3N4 solution with a volume of 10-40μL; 2) The CDs@C3N4 solution was naturally cooled to obtain nitrogen-deficient metal-free flower cluster-like C3N4 photocatalyst.

[0008] Furthermore, the mass of urea is 10 g, the heating temperature is 550° C., and the reaction time is 3 h.

[0009] The present invention also provides the use of the nitrogen-deficient metal-free flower cluster C3N4 photocatalyst in the degradation of tetracycline antibiotics.

[0010] The specific method is as follows: the activity of C3N4 photocatalytic degradation of tetracycline antibiotics is tested under xenon lamp simulated sunlight conditions, a tetracycline antibiotic solution with a concentration of 20 mg / L is taken for photocatalytic degradation, the experimental temperature is controlled at 25°C, 0.1-0.9 g / L nitrogen-deficient metal-free flower cluster C3N4 photocatalyst is dispersed in 50 mL tetracycline antibiotic aqueous solution, the initial pH value of the solution is controlled to be 2-10, and the solution is stirred at a speed of 500 rpm with a magnetic stirrer in a dark environment, and the adsorption and desorption equilibrium is reached after 30 minutes; the system is subjected to a light irradiation experiment, and 3 mL of the reaction suspension is taken every 5 minutes under irradiation of 320nm-780nm, and the remaining photocatalyst particles are immediately removed by filtration with a 0.22 µm polyethersulfone membrane; the absorbance of the TCH solution is detected at the maximum absorption wavelength of λ=357nm, and the concentration of tetracycline antibiotics in the solution is analyzed and determined to obtain the degradation rate, and the degradation rate is calculated as follows: , η is the degradation rate, C0 is the concentration of the wastewater solution before the reaction, C t is the concentration of the wastewater solution at reaction time t.

[0011] Furthermore, the dosage of the nitrogen-deficient metal-free clustered C3N4 photocatalyst is 0.5 g / L; and the initial pH value of the solution is controlled to be 4.

[0012] Furthermore, the tetracycline antibiotic is any one of tetracycline hydrochloride TCH, chlortetracycline hydrochloride CTC, and oxytetracycline OTC.

[0013] The novel nitrogen-deficient metal-free flower cluster photocatalyst prepared by the method of the present invention effectively increases the specific surface area of ​​C3N4, promotes the separation of electron-hole pairs, enhances the photocatalytic performance of C3N4, and can be used for photocatalytic efficient removal of tetracycline antibiotics.

[0014] Compared with the prior art, the present invention has simple operation steps and low price, and the prepared semiconductor catalyst does not contain metal, is environmentally friendly, and does not cause secondary pollution to the environment. The prepared catalyst can be reused many times, and can efficiently remove tetracycline antibiotics in a short time, with a removal rate of more than 98%. The new metal-free flower cluster photocatalyst expands the specific surface area of ​​the C3N4 catalyst, improves the separation of electron-hole pairs, and reduces the mass transfer resistivity, thereby effectively promoting the photocatalytic effect of C3N4. The prepared introduction of metal-free flower cluster C3N4 provides a new design strategy for the preparation of efficient photocatalysts and provides a new idea for the rapid and efficient degradation of tetracycline antibiotics.

[0015] The present invention uses density functional theory analysis and calculation (DFT) to calculate the reaction mechanism of C3N4 photocatalytic removal of tetracycline antibiotics. It may be due to the nitrogen defects in C3N4 that can effectively regulate the recombination of excitons, promote the separation of electron-hole pairs, and form holes h + , •O2 - and 1 O2 effectively enhanced the photocatalytic performance of C3N4.

[0016] In summary, the present invention has a simple operating process, economical and cheap raw materials, stable performance of the obtained catalyst, and good catalytic effect, which solves the problem that the existing C3N4 preparation method cannot be mass-produced due to process and raw material limitations. Under simulated sunlight conditions, the removal rate of tetracycline antibiotics by C3N4 reached more than 98% within 60 minutes. Compared with the typical M-C3N4, C3N4 exhibits excellent photocatalytic activity. The prepared C3N4 shows excellent photocatalytic activity in the degradation of tetracycline antibiotics. At the same time, after being reused 4 times, more than 85% of tetracycline antibiotics are still removed, indicating that the material has good repeatability and stability. In addition, both free radical quenching experiments and density functional theory calculations show that the photocatalytic process of C3N4 is mainly through superoxide radicals. 1 O2, •O2 - and h + The novel photocatalyst prepared by the present invention and the establishment of an effective method for degrading tetracycline antibiotics provide a new idea. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The transmission electron microscope image and scanning electron microscope image of C3N4 prepared in Example 1; in the figure: A is the SEM image of C3N4; B is the TEM image of C3N4; Figure 2 The detection spectrum of C3N4 prepared in Example 1, in which: A is the XRD pattern of C3N4; B is the FT-IR pattern of C3N4; C is the XPS spectrum of C3N4; D is the C1s pattern; E is the N1s pattern; F is the O1s high-resolution spectrum; Figure 3 The fluorescence emission spectrum and ultraviolet absorption spectrum of C3N4 prepared in Example 1 and M-C3N4 prepared in Experimental Example 1; A in the figure is the fluorescence emission spectrum; B is the ultraviolet absorption spectrum; Figure 4The photocatalytic degradation diagram of TCH by C3N4 prepared in Example 1 and M-C3N4 prepared in Experimental Example 1; in the figure: A is the photocatalytic degradation of TCH by C3N4 and M-C3N4; B is the effect of different C3N4 catalyst amounts on TCH degradation; C is the effect of C3N4 catalyst on TCH degradation at different pH; D is the cyclic stability test of C3N4 photocatalyst; E is the dark adsorption diagram of TCH by C3N4 and M-C3N4; F is the adsorption and desorption diagram of C3N4 and M-C3N4; Figure 5 In the figure, A is the PL spectra of C3N4 and M-C3N4; B is the UV-Vis DRS spectra of C3N4 and M-C3N4; C is the band structure diagram of C3N4 and M-C3N4; D is the FT-IR spectrum of C3N4 and M-C3N4CN and PCN; E is the XPS measurement spectrum of C3N4 and M-C3N4; F is the effect of different free radical quenchers on the catalytic degradation of TCH by C3N4; Figure 6 The diagram is the mechanism of TCH degradation by C3N4; Figure 7 In the figure, A is the hole and electron distribution of C3N4 in the S1 state; B is the hole and electron distribution of M-C3N4 in the S1 state, green represents the area that receives electrons, and blue represents holes; C is the Gibbs free energy diagram of C3N4 and M-C3N4; Figure 8 This is a photocatalytic degradation diagram of C3N4 prepared in Example 1 on tetracycline antibiotics, namely chlortetracycline hydrochloride (CTC) and oxytetracycline (OTC). DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and the disclosure and materials cited therein are hereby incorporated by reference.

[0020] Technical equivalents to the specific embodiments described that are apparent to those skilled in the art using no more than routine experimentation are intended to be encompassed by this application.

[0021] The experimental methods in the following examples are all conventional methods unless otherwise specified. The instruments and equipment used in the following examples are all conventional laboratory instruments and equipment unless otherwise specified; the experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.

[0022] Example 1: A nitrogen-deficient metal-free flower cluster C3N4 photocatalyst is prepared by thermal polymerization using single urea as a precursor. The specific steps are as follows: (1) Weigh 10 g of urea and place it in a reactor, then add 10 mL of secondary aqueous solution, stir thoroughly, and ultrasonicate for 5 min to obtain a clear solution; place the reactor containing the clear solution in an oven to dry, then place it in a muffle furnace and heat it to 550 °C at a heating rate of 10 °C / min for 3 h; (2) The above reaction product is taken out of the reactor and cooled naturally to obtain the target product C3N4.

[0023] Example 2: A nitrogen-deficient metal-free cluster C3N4 photocatalyst. 8 g of urea is placed in a reactor, followed by the addition of 10 mL of a secondary aqueous solution. The remaining steps are the same as those described in Example 1. The reaction product is taken out of the reactor and cooled naturally to obtain the target product C3N4-1.

[0024] Example 3: A nitrogen-deficient metal-free cluster C3N4 photocatalyst, 12g of urea is placed in a reactor, and then 10mL of a secondary aqueous solution is added; the rest of the method is the same as that described in Example 1, the above reaction product is taken out of the reactor, cooled naturally, and the target product C3N4-2 is obtained.

[0025] Example 4: A nitrogen-deficient metal-free cluster C3N4 photocatalyst, 10g of urea is placed in a reactor, then 10mL of secondary aqueous solution is added, and the reactor is placed in a muffle furnace and heated to 500°C at a heating rate of 10°C / min for 2h; the rest of the method is the same as that described in Example 1, the reaction product is taken out of the reactor, cooled naturally, and the target product C3N4-3 is obtained.

[0026] Example 5: A nitrogen-deficient metal-free cluster C3N4 photocatalyst, 10g of urea is placed in a reactor, followed by adding 10mL of a secondary aqueous solution, and then placed in a muffle furnace and heated to 600°C at a heating rate of 10°C / min for 4h; the rest of the method is the same as that described in Example 1, the above reaction product is taken out of the reactor, cooled naturally, and the target product of C3N4-4 is obtained.

[0027] Experimental Example 1: 10 g of melamine was weighed and placed in a reactor, which was then placed in a muffle furnace and heated to 550° C. for 3 h. The reaction product was taken out of the reactor and cooled naturally to obtain the target product M-C3N4.

[0028] The performance of C3N4 and M-C3N4 prepared in Examples 1-5 and Experimental Example 1 was characterized and tested. The results are shown in Figure 1-4 , the degradation mechanism and pathway results are shown in 5-9.

[0029] Morphology analysis: In order to observe the surface morphology of C3N4, SEM and TEM were used to analyze its characteristics, such as Figure 1 As shown, the morphology of C3N4 was analyzed and characterized by SEM. Figure 1 As shown in Figure A, C3N4 has a flower cluster-like porous sheet structure and is relatively fluffy. This is because urea decomposes rapidly under high temperature, producing a large amount of NH3, which makes its structure fluffy and thin, increasing its specific surface area. In the intermediate process of preparing C3N4, the early intermediate product is melamine. As the temperature rises further, melamine will thermally polymerize to form carbon nitride. TEM is used to conduct a more in-depth analysis and characterization of the morphology of C3N4, and the surface is flat and dense. Figure 1 It can be clearly observed in Figure 2B that the prepared C3N4 has a very thin thickness and a larger specific surface area due to the agitation of NH3, which may be more conducive to the further photocatalytic degradation process.

[0030] XRD analysis: The crystal structure of C3N4 was analyzed and characterized by XRD, such as Figure 2 As shown in A, C3N4 has two obvious peaks, both of which belong to the typical C3N4 structural diffraction peaks. Among them, the diffraction peak at 27° belongs to the characteristic diffraction peak of the C3N4 (002) crystal plane, which is caused by the interlayer stacking of conjugated aromatic sheets. The peak at 13° is the characteristic diffraction peak of the C3N4 (100) crystal plane, corresponding to the stacking between N holes in the basic unit of its heptazine ring structure.

[0031] Surface functional group and elemental composition analysis: FT-IR and XPS analysis are used to infer the molecular structure and chemical functional groups of the compounds. FT-IR is used to analyze the characteristic spectrum or fingerprint area of ​​C3N4 to determine the type of functional groups contained in these compounds and their chemical environment, such as Figure 2 As shown in B, C3N4 is between 3500 and 3000 cm - The wide characteristic absorption peaks in the range of 1200-1700 cm-1 are related to the NH bonds in the amino groups that are not completely polymerized on the surface of C3N4 and the OH stretching vibrations in the hydroxyl-containing substances. - The absorption peak of the ¹ band is caused by the CN and C=N stretching vibrations on the C3N4 heterocycle. - The fingerprint absorption peak at ¹ belongs to the characteristic vibration peak of the triazine ring structural unit.

[0032] In order to further describe the surface composition and chemical structure of C3N4, C3N4 was further analyzed by XPS, such as Figure 2 As shown in Figure C, the electron energy peaks of C, N and O in C3N4 are located at 283.99 eV, 398.1 eV and 531.78 eV, respectively. The percentages of C, N and O calculated by integration are 46.42%, 49.95% and 3.63%, respectively. The C1s high-resolution spectrum (2D) of C3N4 fits three peaks, located at 284.70 eV, 286.28 eV and 288.41 eV, respectively. The peak position of 284.70 eV belongs to the graphite carbon structure, the peak position of 286.28 eV belongs to the carbon skeleton and hydroxyl group (C-OH), and the peak position of 288.41 eV belongs to the triazine ring carbon (NC=N). Figure 2 E shows the high-resolution spectrum of N1s. The N1s of C3N4 is fitted with four peaks, belonging to C=NC (398.58 eV), C-N3 (399.78 eV), NH (401.73 eV) and graphite-N (403.21 eV). Figure 2 The O1s high-resolution spectrum of C3N4 in F shows two peaks, which are attributed to the OH bond (531.50 eV) and the C=O bond (533.20 eV). The above XPS characterization results are consistent with the FT-IR analysis results.

[0033] Further FT-IR analysis showed that the NH stretching peak (3150-3600cm) of M-C3N4 prepared from melamine was higher than that of C3N4 prepared from urea. -1 ) is strong, and the asymmetric stretching vibration of cyano (N≡C-) (2147cm -1 ) is weak. This further indicates that the concentration of -NH2 groups in C3N4 prepared with urea as raw material is reduced, and the concentration of cyano (N≡C-) functional groups is enhanced, making C3N4 have more abundant nitrogen defects, which can act as shallow charge traps to accelerate the efficiency of charge transfer. In addition, the nitrogen content of C3N4 in the XPS elemental analysis results (5E) is less than that of M-C3N4, further confirming the above results.

[0034] Optical performance analysis: In order to analyze the optical properties of C3N4, fluorescence spectroscopy and UV-visible spectroscopy were used for analysis and characterization. Figure 3 As shown in A, the optimal excitation wavelength and emission wavelength of C3N4 are 300nm and 440nm respectively. The UV-visible absorption spectrum of C3N4 is shown in Figure 3 As shown in Figure B, it can be seen from the figure that C3N4 has obvious absorption peaks at 233nm and 332nm, which are caused by the π→π* transition and n→π* transition of C=O respectively.

[0035] Experimental Example 2: The photocatalyst prepared in the embodiment is used for photocatalytic efficient removal of tetracycline antibiotics (here tetracycline (TCH) is mainly used as the research object), and the activity of C3N4 photocatalytic degradation of TCH is tested under xenon lamp simulated sunlight conditions. Take a concentrated TCH solution (20 mg / L) for photocatalytic degradation, detect the absorbance of the TCH solution at the maximum absorption wavelength of λ=357 nm, and calculate its degradation rate. The specific operation steps are as follows: Take the photocatalyst obtained in the embodiment, weigh the C3N4 photocatalyst (0.5 g / L) and disperse it in 50 mL of tetracycline antibiotic aqueous solution, and stir it with a magnetic stirrer at a speed of 500 r / min in a dark environment. After 30 minutes, the adsorption and desorption equilibrium is reached (the experimental temperature is 25°C). The system is subjected to a light irradiation experiment. Every 5 minutes, 3 mL of the reaction suspension is taken and immediately filtered with a 0.22 µm polyethersulfone membrane to remove the remaining photocatalyst particles. The concentration of tetracycline antibiotics in the solution was determined by UV-visible spectrophotometer, where the initial concentration of the tetracycline antibiotic solution was C0 and the sampling concentration during the degradation process was C t The photocatalytic degradation rate (η) of TCH can be calculated as follows: ; Where η is the degradation rate of simulated wastewater, C0 is the concentration of wastewater solution before reaction, C t is the concentration of the wastewater solution at reaction time t.

[0036] The results are as follows Figure 4 As shown in A, at 20 min, the degradation of TCH by C3N4 can reach 98.44%, and at 60 min, the degradation is as high as 99.60%. The catalyst with the best degradation efficiency was screened, among which the degradation efficiency in Example 1 was the highest, up to 99.60%.

[0037] Experimental Example 3: The effects of factors such as the dosage of C3N4 and the initial pH value of the solution on the degradation of TCH were further investigated. Figure 4 is the photocatalytic degradation diagram, Figure 4 B shows that when the dosage of C3N4 is 0.1 g / L, 0.3 g / L, 0.5 g / L, 0.7 g / L and 0.9 g / L, the photocatalytic degradation of TCH is 91.78%, 98.46%, 99.58%, 99.64% and 99.41% respectively; with the increase of C3N4 dosage, the degradation efficiency gradually increases, but after increasing to 0.5g / L, the photocatalytic degradation effect of TCH has basically not changed, which may be due to the increase of solid particle concentration in the solution with the increase of catalyst concentration, which affects the absorption of light by the catalyst, thereby reducing the photocatalytic performance. In summary, 0.5g / L of catalyst is selected as the best catalyst dosage.

[0038] In order to study the effect of the initial pH value of the solution on the photocatalytic degradation of TCH, photocatalytic degradation experiments were carried out at pH values ​​of 2.0, 4.0, 6.0, 8.0, and 10.0. The results are shown in Figure 2. Figure 4 As shown in Figure C, the initial pH value has a certain degree of influence on the degradation rate of TCH photodegradation by C3N4. As the pH decreases, the catalytic degradation of TCH by C3N4 gradually increases, that is, when the pH is alkaline, the catalytic effect decreases. When pH=10, the degradation rate of TCH is as low as 86.81%, which may be related to the change in pH value leading to changes in the surface morphology or charge distribution of the photocatalyst. pH=4 is selected as the optimal value.

[0039] Experimental Example 4: In order to evaluate the stability of the C3N4 photocatalyst, a C3N4 recycling experiment was carried out under xenon lamp irradiation simulating sunlight. Figure 4 D is a cyclic experiment of C3N4 photocatalytic degradation of TCH. After C3N4 was repeatedly recycled for 4 times, the degradation rates were 99.27%, 98.60%, 98.59% and 98.43%, respectively, and the degradation effect remained above 98%. The experimental results show that the C3N4 photocatalyst has good repeatability and stability and can be recycled many times.

[0040] Experimental Example 5: Analysis of the photocatalytic degradation mechanism of tetracycline antibiotics: In order to further study the catalytic mechanism of C3N4, a catalyst carbon nitride (M-C3N4) was prepared using melamine as a single raw material as a comparative experiment. Figure 4 As shown in A, under the same conditions, using M-C3N4 as the photocatalyst, the degradation of TCH was 63.55% in 20 min and 93.39% in 60 min. By comparison, it was found that the photocatalytic performance of C3N4 on TCH was indeed much better than that of M-C3N4. This difference may be due to the fact that C3N4 has a larger specific surface area, more abundant active sites, more nitrogen defects and a faster mass transfer rate than M-C3N4.

[0041] In order to further verify the above speculation, dark adsorption contrast experiments were carried out. Figure 4 In E, the removal rate of TCH by M-C3N4 in the dark reaction stage is about 1.13%, and the removal rate of TCH by C3N4 is 5.96%. This result confirms that the surface area of ​​C3N4 is larger than that of M-C3N4. The specific surface areas of C3N4 and M-C3N4 were further tested and analyzed by BET nitrogen adsorption experiment. According to the N2 adsorption and desorption isotherms of C3N4 and M-C3N4 ( Figure 4 F), the specific surface area of ​​C3N4 (72.339 m 2 / g) is much higher than M-C3N4 (3.773 m 2 / g). This may be because urea produces a large amount of gas due to high temperature during the preparation process, resulting in a fluffy structure and a thin thickness, which effectively increases its specific surface area, making C3N4 have a wider surface space, thereby providing more catalytic active sites and promoting the photocatalytic degradation of TCH.

[0042] During the photocatalytic reaction, photoluminescence (PL) is an effective method to characterize the photogenerated carrier separation ability of photocatalysts. As the fluorescence intensity decreases, the photogenerated carrier separation ability of photocatalysts increases. Based on this, the PL intensities of C3N4 and M-C3N4 were compared. The characteristic peaks of fluorescence emission of C3N4 and M-C3N4 are both located near 440 nm, but the PL intensity of C3N4 (5606.37 au) is much lower than that of M-C3N4 (27233.25 au) ( Figure 5 As shown in A), it further illustrates that C3N4 prepared based on urea has a higher separation efficiency of photogenerated carriers.

[0043] To gain a deeper understanding of the photocatalytic activity of C3N4, the electronic structure of C3N4 was studied. Figure 5 As shown in B, the band gap was analyzed by ultraviolet-visible light (UV-vis) absorption spectroscopy. C3N4 showed an intrinsic absorption edge near 460nm. The band gap was calculated to be about 2.75eV based on the Kubelka-Munk function. M-C3N4 had a similar absorption edge with a band gap of about 2.69eV. C3N4 and M-C3N4 were further tested by electrochemical Mott-Schottky. The flat band potentials of C3N4 and M-C3N4 were -0.59 eV and -0.65 eV (V vs. AgCl). According to E NHE =E(Ag / AgCl)+0.197Calculate the conduction band potential of C3N4 and M-C3N4 (E CB ) are: -0.39 and -0.65 eV (V vs. NHE) According to the formula Eg=E VB -E CB , the valence bands (VB) of C3N4 and M-C3N4 catalysts were calculated to be 2.36 eV and 2.04 eV (relative to NHE), respectively. The detailed band structure scheme is shown in Figure 5 C, this result shows that C3N4 has a deeper valence band, better oxidation effect and catalytic activity, and better catalytic degradation effect on TCH. Since the slope of the Mott-Schottky curve fitting line graph is positive, it shows that the catalyst has n-type semiconductor characteristics.

[0044] Further analysis by FT-IR revealed Figure 5As shown in D, compared with C3N4 prepared from urea, the NH stretching peak (3150-3600cm -1 ) is strong, and the asymmetric stretching vibration of cyano (N≡C-) (2147cm -1 ) is weak, further indicating that the concentration of -NH2 groups in C3N4 prepared with urea as raw material is reduced, and the concentration of cyano (N≡C-) functional groups is enhanced, making C3N4 have more abundant nitrogen defects, which can act as shallow charge traps and accelerate the efficiency of charge transfer. In addition, the nitrogen content of C3N4 in the XPS elemental analysis results (5E) is less than that of M-C3N4, further confirming the above results.

[0045] The free radical capture experiment in the photocatalytic reaction is crucial for inferring the mechanism of the photocatalytic reaction. Different capture agents are added to the reaction solution to remove the corresponding free radical reaction active substances, and then the role of different free radical reaction active substances in the photocatalytic process is judged according to the degradation rate of pollutants by photocatalysis. Tert-butanol (TBA) is selected to capture hydroxyl radicals (•OH), p-benzoquinone (p-BQ) to capture superoxide radicals (•O2 ˉ ), Furfuryl Alcohol (FFA) captures singlet oxygen ( 1 O2) and EDTA-2Na (ethylenediaminetetraacetic acid disodium salt) to capture holes (h + ).like Figure 5 As shown in F, after adding different scavengers and 30 min dark adsorption treatment, the photocatalytic degradation effect of C3N4 on TCH was observed. When p-BQ, FFA, EDTA-2Na and TBA scavengers were added, the photocatalytic degradation rate of TCH decreased to 40.21%, 75.68%, 89.93% and 98.05%, respectively. It can be seen that •OH, •O2 ˉ , 1 O2 and H + It has an effect on the photocatalytic degradation of TCH, among which •O2 ˉ , 1 O2 and H + It is the main active substance affecting TCH degradation.

[0046] The photocatalytic degradation mechanism of tetracycline antibiotics by C3N4 is shown in the figure Figure 6As shown, first, under the irradiation of xenon lamp simulated light, C3N4 is excited under light with a wavelength of less than 459nm, and the excited electrons are excited from the valence band (VB) of C3N4 to the conduction band (CB), leaving the corresponding h + VB (Reaction (1)). Secondly, the electrons in the conduction band of C3N4 (e - CB ) reacts with dissolved oxygen in the solution to generate 1 O2 and •O2 ˉ (Reaction (2)). Then, •O2 ˉ Combines with water to form OH and OH ˉ (Reaction (3)). Finally, the generated 1 O2, •O2 ˉ 、h + Both OH and •OH participate in the degradation reaction of TCH (reaction equation (4)). Among them, cyano group acts as a charge trap, which can effectively accelerate the efficiency of charge transfer, and because cyano group can capture holes as the main reaction site for catalytic degradation of TCH. The specific reaction equation is as follows: (1) C3N4+hv→e - CB + h + VB ; (2) O2+e - CB → 1 O2+•O2 ˉ ; (3) 2H2O+•O2 ˉ →2OH ˉ +2•OH; (4) 1 O2,•O2 ˉ ,h + ,•OH+TCH→Products.

[0047] In order to further understand the degradation mechanism of C3N4 photocatalysis, the corresponding energy level diagrams of different excited states were analyzed and calculated in combination with DFT theoretical calculations. Figure 7 It can be found in A that with the increase of cyano groups, the relevant energy level becomes lower, and the electron-hole distribution can be clearly observed. Among them, defects such as cyano groups act as electron acceptors, changing the original electron-hole distribution and providing electron-holes for the 3π-π* state of charge transfer, which may be mixed with some local excitation characteristics. The Gibbs free energy ( Figure 7B) shows that the Gibbs free energy of C3N4 with more defects (0.46 eV) is significantly lower than that of M-C3N4 without nitrogen atoms (0.71 eV). In addition, the Coulomb attraction energy of electrons and holes (Table 1) also shows a trend of decreasing with the increase of nitrogen defects, which further indicates that electron-hole pairs are more likely to dissociate and form free carriers, making it easier to undergo photocatalytic degradation reactions. The above calculation results are consistent with the experimental results.

[0048] Table 1 Coulomb attraction energy between electrons and holes Experimental Example 6: Photocatalytic degradation of tetracycline antibiotics Generality: In order to further investigate the catalytic effect of the prepared C3N4 on tetracycline antibiotics, CTC and OTC were selected as target pollutants. Under the same conditions as the above experiment, the degradation of CTC and OTC was carried out. The results are as follows: Figure 8 As shown in the figure, the degradation rates are 98.80% and 98.29%, respectively. This further shows that the prepared porous flower cluster C3N4 has a good catalytic degradation effect on tetracycline antibiotics, and the degradation rate of tetracycline antibiotics can reach more than 98% within 60 min, indicating that C3N4 is a very potential catalyst.

[0049] The novel metal-free flower cluster C3N4 photocatalyst prepared by the method of the present invention has a larger specific surface area, effectively improves its light absorption capacity, promotes the separation of electron-hole pairs, enhances the photocatalytic performance of C3N4, and can be used for photocatalytic efficient removal of tetracycline antibiotics.

[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A nitrogen-deficient metal-free flower-like C3N4 photocatalyst, characterized in that: Using single urea as precursor, nitrogen-deficient metal-free flower cluster-like C3N4 photocatalyst was prepared by thermal polymerization reaction at 500-600℃ for 2-4h.

2. A method for preparing the nitrogen-deficient metal-free flower cluster C3N4 photocatalyst according to claim 1, characterized in that: The specific method is: 1) 8-12g urea was added with 10ml secondary water, stirred thoroughly, and ultrasonicated for 5min to obtain a clear solution; the clear solution was dried at 100℃ for 6h, and then heated to 500-600℃ at a heating rate of 10℃ / min and continued to react for 2-4h to obtain a CDs@C3N4 solution with a volume of 10-40μL; 2) The CDs@C3N4 solution was naturally cooled to obtain nitrogen-deficient metal-free flower cluster-like C3N4 photocatalyst.

3. The preparation method according to claim 2, characterized in that: The mass of urea is 10 g, the heating temperature is 550°C, and the reaction time is 3 h.

4. Use of the nitrogen-deficient metal-free flower cluster C3N4 photocatalyst according to claim 1 in the degradation of tetracycline antibiotics.

5. The use according to claim 4, characterized in that: The specific method is as follows: the activity of C3N4 photocatalytic degradation of tetracycline antibiotics is tested under xenon lamp simulated sunlight conditions, a tetracycline antibiotic solution with a concentration of 20 mg / L is taken for photocatalytic degradation, the experimental temperature is controlled at 25°C, 0.1-0.9 g / L nitrogen-deficient metal-free flower cluster C3N4 photocatalyst is dispersed in 50 mL tetracycline antibiotic aqueous solution, the initial pH value of the solution is controlled to be 2-10, and the solution is stirred at a speed of 500 rpm with a magnetic stirrer in a dark environment, and the adsorption and desorption equilibrium is reached after 30 minutes; the system is subjected to a light experiment, and 3 mL of the reaction suspension is taken every 5 minutes under irradiation of 320nm-780nm, and the remaining photocatalyst particles are immediately removed by filtration with a 0.22 µm polyethersulfone membrane; the absorbance of the tetracycline antibiotic solution is detected at the maximum absorption wavelength of λ=357nm, and the concentration of tetracycline antibiotics in the solution is analyzed and determined to obtain the degradation rate, and the degradation rate is calculated as follows: , η is the degradation rate, C0 is the concentration of the wastewater solution before the reaction, C t is the concentration of the wastewater solution at reaction time t.

6. The application according to claim 5, characterized in that: The amount of the nitrogen-deficient metal-free flower cluster C3N4 photocatalyst used is 0.5 g / L; the initial pH value of the solution is controlled to be 4.

7. The use according to claim 5, characterized in that: The tetracycline antibiotic is any one of tetracycline hydrochloride TCH, chlortetracycline hydrochloride CTC, and oxytetracycline OTC.

Citation Information

Patent Citations

  • Protonated g-C3N4 / BiOBr heterojunction photocatalyst and preparation method

    CN109092342A

  • Preparation method of g-C3N4 catalyst for degrading tetracycline

    CN117680180A

Cited By

  • Homojunction photocatalyst as well as preparation method and application thereof

    CN120205210A

  • Antibiotic-polluted underground water remediation method based on Fe / Nv-PCN piezoelectric material

    CN120208358A