Cu / S in-situ co-doped high-crystallinity carbon nitride monatomic catalyst as well as preparation method and application thereof
Through the preparation of Cu/S in situ co-doped high-crystalline carbon nitride single-atom catalyst, the problems of low utilization rate and poor stability of heterogeneous Fenton catalysts in H2O2 are solved, and efficient degradation of organic pollutants is achieved, especially High activity and stability are shown in the photofenton reaction of sulfonamides.
Patent Information
- Application Number
- CN202411290805.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-22
AI Technical Summary
The existing heterogeneous Fenton catalysts have low H2O2 utilization rate, low Fenton activity and poor stability. The preparation process of one-step and step-by-step methods is complicated and costly, making it difficult to ensure the uniformity of the precursor, which affects the impact of Catalyst performance.
The preparation method of Cu/S in situ co-doped high-crystalline carbon nitride single-atom catalyst is adopted. Through supramolecular self-assembly and thermal polymerization, the coordination effect of Cu2+ with melamine and trimeric thiocyanic acid is used to combine molten salt heat. Polymerization achieves uniform doping of Cu and S, forming a high crystalline carbon nitride structure, and improving photofenton activity and stability.
The preparation of Cu/S in situ co-doped high-crystalline carbon nitride single-atom catalyst with simple operation and low cost is realized. It has high light Fenton activity and stability, and can effectively degrade organic pollutants, especially for sulfamethoxazole. Organic pollutants such as sulfamethrin, ciprofloxacin, norfloxacin, and tetracycline have excellent degradation effects.
Smart Images

Figure CN118988378A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst and a preparation method and application thereof, and specifically to a Cu / S in-situ co-doped high-crystalline carbon nitride single-atom catalyst and a preparation method and application thereof. Background Art
[0002] Fenton oxidation technology can efficiently degrade organic pollutants by producing highly reactive reactive oxygen species. It has a rapid, efficient and easy-to-operate reaction, and is therefore widely used in the field of sewage treatment. However, the traditional homogeneous Fenton system has disadvantages such as a narrow pH range of use and the production of a large amount of iron-containing sludge. Compared with homogeneous Fenton reaction catalysts, heterogeneous Fenton reactions have the advantages of a wide pH working range and are not prone to secondary pollution. Common heterogeneous Fenton catalysts include transition metal oxides, sulfides, MOFs, etc. However, these heterogeneous Fenton catalysts have defects such as low H2O2 utilization, low Fenton activity and poor stability.
[0003] Carbon nitride is a typical organic non-metallic semiconductor photocatalytic material with a suitable band gap and energy band structure, and has the advantages of low preparation cost, simple synthesis method, and good stability. Therefore, transition metals with Fenton activity can be incorporated into the carbon nitride matrix to prepare heterogeneous photo-Fenton catalysts. In addition, since the photogenerated carrier separation efficiency of carbon nitride itself is low, its photo-Fenton activity can be further improved by non-metallic doping. Therefore, doping the carbon nitride matrix with metal and non-metal atoms at the same time can significantly improve the photo-Fenton activity of carbon nitride.
[0004] At present, the preparation of metal and non-metal atom co-doped carbon nitride mainly includes a one-step method and a step-by-step method. The step-by-step method refers to the step-by-step doping of metal and non-metal into the carbon nitride precursor. The Chinese patent with the authorization number CN115970731B discloses a method for step-by-step doping of metal and non-metal atoms in carbon nitride: first, melamine and non-metal heteroatom precursors (boron oxide, ammonium dihydrogen phosphate or thioacetamide) are prepared by thermal polymerization and alkali metal intercalation to prepare non-metal atom doped carbon nitride, and then the transition metal is further doped into the carbon nitride by an impregnation method to prepare a non-metal doped substrate-loaded metal single atom catalyst. The preparation step is divided into a non-metal heteroatom doping process and a metal single atom loading process, and the preparation process is complicated and cumbersome with high cost. At the same time, the preparation process requires a large amount of organic solvent (N-methylpyrrolidone / ethanol), which faces the problems of high pollution and high cost. In addition, the heteroatom monomer may introduce other elements into the carbon nitride during the pyrolysis process. One-step method refers to the simultaneous incorporation of metal and non-metal into carbon nitride, and carbon nitride precursor, metal precursor and non-metal precursor are usually mixed and prepared by thermal polymerization reaction. The Chinese patent with the authorization number CN109772423B is a phosphorus and bismuth co-doped porous graphite phase carbon nitride photocatalyst and its use. Non-metallic P and metal Bi are co-doped carbon nitride, which is mainly through urea, hexachlorocyclotriphosphazene and bismuth nitrate grinding and then thermal polymerization. Although the preparation process is simple, it is difficult to ensure uniform mixing because the precursor is only physically mixed. The Chinese patent with the authorization number CN116328814B is an easily separable nickel and boron doped carbon nitride catalyst and its preparation method, and a method for simultaneously incorporating non-metallic B and transition metal Ni into carbon nitride. It is mainly to dissolve nickel salt, boric acid and urea in water, dry to obtain a mixed precursor, and then prepare a nickel and boron doped carbon nitride catalyst by pyrolysis of the precursor. The process obtains a mixed precursor by drying the precursor solution, and it is still difficult to ensure uniformity.
[0005] Therefore, for the one-step method, it is difficult to mix the three precursors evenly by simple physical mixing, making it difficult to maintain stable performance of the prepared material, thus affecting its catalytic activity. Summary of the invention
[0006] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst which is simple to operate and low in cost. Another purpose of the present invention is to provide a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst with high photo-Fenton activity and good stability. A further purpose of the present invention is to provide an application of a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst in the degradation of sulfamethoxazole, sulfamethoxazole, ciprofloxacin, norfloxacin, tetracycline, and oxytetracycline in wastewater.
[0007] Technical solution: The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst according to the present invention comprises the following steps:
[0008] Step 1, mixing melamine, thiocyanate and copper salt in water and heating, cooling, filtering and drying to obtain a copper-loaded supramolecular precursor;
[0009] Step 2, subjecting the copper-loaded supramolecular precursor to a thermal polymerization reaction under protective gas conditions to obtain Cu / S in-situ co-doped low-crystalline carbon nitride;
[0010] Step three, after mixing the Cu / S in-situ co-doped low-crystalline carbon nitride and the molten salt, a secondary thermal polymerization reaction is carried out under protective gas conditions. After washing with water, filtering and drying, the Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst can be obtained.
[0011] Furthermore, in step 1, the molar ratio of melamine, thiocyanate and copper salt is 100:100:1-20. The copper salt is one or more of CuCl2, CuSO4, Cu(NO3)2, Cu(CH3COO)2. The heating temperature is 30-100°C and the heating time is 2-8h.
[0012] Furthermore, in step 2, the temperature of the first thermal polymerization reaction is 500-600° C., the time of the first thermal polymerization reaction is 1-8 hours, and the heating rate is 1-10° C. / minute.
[0013] Furthermore, in step 3, the molten salt is one or more of KCl, LiCl, and NaCl. The mass ratio of Cu / S co-doped low-crystalline carbon nitride to the molten salt is 1:1 to 20. The temperature of the secondary thermal polymerization reaction is 450 to 650°C, and the time of the secondary thermal polymerization reaction is 1 to 6 hours. The heating rate is 1 to 10°C / minute.
[0014] Furthermore, the protective gas includes Ar or N2.
[0015] The Cu / S in-situ co-doped high-crystalline carbon nitride single-atom catalyst prepared by the method for preparing the Cu / S in-situ co-doped high-crystalline carbon nitride single-atom catalyst of the present invention comprises the following substances in percentage by weight: S 0.09wt% to 0.32wt%, Cu 0.1wt% to 10wt%, and the rest being carbon nitride; the carbon nitride is poly(heptazineimide, PHI), Cu is doped in the pores of the carbon nitride in the form of single atoms, and S is located on the skeleton of the carbon nitride in the form of substitutional doping.
[0016] The Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst of the present invention is used in photo-Fenton degradation of sulfamethoxazole, sulfamethoxazole, ciprofloxacin, norfloxacin, tetracycline and oxytetracycline in wastewater.
[0017] Preparation principle: Using Cu 2+ The copper-loaded supramolecular precursor is self-assembled through the coordination and hydrogen bonding between thiocyanate and melamine. The S / Cu in-situ co-doped low-crystalline carbon nitride is prepared by pyrolysis of the copper-loaded supramolecular precursor. Finally, the S / Cu in-situ co-doped carbon nitride is converted into S / Cu in-situ co-doped high-crystalline carbon nitride through a molten salt thermal polymerization process. Cu acts as a photo-Fenton reaction center, and S-doped high-crystalline carbon nitride improves the separation efficiency of photogenerated carriers. Therefore, the Cu / S in-situ co-doped high-crystalline carbon nitride single-atom catalyst has high photo-Fenton activity.
[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0019] 1. The prepared material has the advantages of high photo-Fenton activity and good stability. The Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst is used to treat a certain concentration of aqueous solution of organic pollutants. When a small amount of H2O2 is added, it can effectively photocatalytically activate H2O2 to degrade organic pollutants in the solution;
[0020] 2. The Cu single atom site acts as the Fenton reaction center, and S-doped highly crystalline carbon nitride improves the efficiency of photogenerated carrier separation. The uniform distribution of the two can effectively play a synergistic role;
[0021] 3. The operation is simple and the cost is low. Through the supramolecular self-assembly process of the precursor, Cu and S are evenly dispersed in the precursor. Then, through two thermal polymerization processes, Cu and S are simultaneously and evenly doped in situ in the highly crystalline carbon nitride structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a cycle performance diagram of the photo-Fenton degradation of sulfamethoxazole by Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention;
[0023] Figure 2 This is a performance diagram of photo-Fenton degradation of sulfamethoxazole by Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) under different inorganic salt conditions in Example 2 of the present invention;
[0024] Figure 3 This is a performance diagram of Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in photo-Fenton degradation of different organic pollutants in Example 2 of the present invention;
[0025] Figure 4The Cu-loaded supramolecular precursor (Cu x -TMCA, x = 0.1, 0.3, 0.5, 1 and 2) and the XRD pattern of the supramolecular precursor (TMCA) in Comparative Example 1;
[0026] Figure 5 The Cu-loaded supramolecular precursor (Cu 0.3 -TMCA) and the solid UV-visible diffuse reflection absorption spectra of the supramolecular precursor (TMCA) in Comparative Example 1;
[0027] Figure 6 The Cu-loaded supramolecular precursor (Cu 0.3 -TMCA) scanning electron microscopy images;
[0028] Figure 7 XRD patterns of Cu / S co-doped highly crystalline carbon nitride (CuSCCN-x, x=0.1, 0.3, 0.5, 1 and 2) in Examples 1 to 5 of the present invention and S-doped highly crystalline carbon nitride (SCCN) in Comparative Example 1;
[0029] Figure 8 TEM and HRTEM images of Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention, wherein (a) is a TEM image and (b) is a HRTEM image;
[0030] Fig. 9 The spherical aberration-corrected transmission electron microscope image and the corresponding element scanning image of the Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention, wherein (a) is a transmission electron microscope image, (b) is a C element scanning image, (c) is an N element scanning image, (d) is a Cu element scanning image, (e) is an S element scanning image, and (f) is a spherical aberration-corrected transmission electron microscope image and the corresponding element scanning image;
[0031] Fig.10 The performance curves of photo-Fenton degradation of sulfamethoxazole by Cu / S co-doped highly crystalline carbon nitride (CuSCCN-x, x=0.1, 0.3, 0.5, 1 and 2) in Examples 1 to 5 of the present invention, S-doped highly crystalline carbon nitride (SCCN) in Comparative Example 1 and Cu-doped highly crystalline carbon nitride (CuSCCN-0.3) in Comparative Example 2;
[0032] Fig.11 The kinetic diagram of photo-Fenton degradation of sulfamethoxazole by Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention and Examples 6 to 11 (CuSCCN-a to h) is shown. DETAILED DESCRIPTION
[0033] The experimental methods described in the examples are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified. XPA-7 photochemical reactor was purchased from Nanjing Xujiang Electromechanical Factory.
[0034] Example 1
[0035] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0036] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added to 200 mL of ultrapure water, and 0.1 mmol of CuCl2 was added. The mixture was stirred in a water bath at 80 °C for 2 h, and then filtered and dried in vacuum to obtain a Cu-loaded supramolecular precursor, which was recorded as Cu. 0.1 -TMCA.
[0037] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-0.1.
[0038] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, recorded as CuSCCN-0.1.
[0039] Application Example 1
[0040] The CuSCCN-0.1 photocatalyst obtained in Example 1 was used to degrade sulfamethoxazole. The specific experimental conditions were: 10 mg of the catalyst was placed in 50 mL of a 20 mg / L tetracycline solution, and adsorption-desorption equilibrium was reached after 30 minutes, and then 50 μL of a H2O2 solution (30 wt%) was added, and a xenon lamp was turned on for a photo-Fenton reaction.
[0041] Example 2
[0042] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0043] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added to 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. The mixture was stirred in a water bath at 80 °C for 2 h, and then filtered and dried in vacuum to obtain the Cu-loaded supramolecular precursor, which was recorded as Cu. 0.3 -TMCA.
[0044] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-0.3.
[0045] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, recorded as CuSCCN-0.3.
[0046] Example 3
[0047] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0048] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added to 200 mL of ultrapure water, and 0.5 mmol of CuCl2 was added. The mixture was stirred in a water bath at 80 °C for 2 h, and then filtered and dried in vacuum to obtain a Cu-loaded supramolecular precursor, which was recorded as Cu 0.5 -TMCA.
[0049] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-0.5.
[0050] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, recorded as CuSCCN-0.5.
[0051] Example 4
[0052] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0053] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water, and 1 mmol of CuCl2 was added. After stirring in a water bath at 80 °C for 2 h, the Cu-loaded supramolecular precursor was obtained after suction filtration and vacuum drying, which was recorded as Cu1-TMCA.
[0054] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-1.
[0055] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-1.
[0056] Example 5
[0057] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0058] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water, and 2 mmol of CuCl2 was added. After stirring in a water bath at 80 °C for 2 h, the Cu-loaded supramolecular precursor was obtained after suction filtration and vacuum drying, which was recorded as Cu2-TMCA.
[0059] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-2.
[0060] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, recorded as CuSCCN-2.
[0061] Example 6
[0062] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0063] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. After stirring in a 30°C water bath for 8 h, the Cu-loaded supramolecular precursor was obtained after suction filtration and vacuum drying.
[0064] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained.
[0065] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-a.
[0066] Example 7
[0067] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0068] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. After stirring in a 100 °C water bath for 2 h, the Cu-loaded supramolecular precursor was obtained after suction filtration and vacuum drying.
[0069] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained.
[0070] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-b.
[0071] Example 8
[0072] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0073] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. After stirring in a water bath at 80 °C for 2 h, the Cu-loaded supramolecular precursor was obtained after suction filtration and vacuum drying.
[0074] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 500 °C for 8 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained.
[0075] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-c.
[0076] Example 9
[0077] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0078] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. After stirring in a water bath at 80 °C for 2 h, the Cu-loaded supramolecular precursor was obtained after suction filtration and vacuum drying.
[0079] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 600 °C for 1 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained.
[0080] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-d.
[0081] Example 10
[0082] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0083] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added to 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. The mixture was stirred in a water bath at 80 °C for 2 h, and then filtered and dried in vacuum to obtain the Cu-loaded supramolecular precursor, which was recorded as Cu. 0.3 -TMCA.
[0084] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-0.3.
[0085] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 450 °C for 6 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-e.
[0086] Embodiment 11
[0087] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0088] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added to 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. The mixture was stirred in a water bath at 80 °C for 2 h, and then filtered and dried in vacuum to obtain the Cu-loaded supramolecular precursor, which was recorded as Cu. 0.3 -TMCA.
[0089] (2) Primary thermal polymerization: Weigh 2 g of the Cu-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, and heat at a rate of 5 °C / min under an Ar atmosphere, and maintain at 550 °C for 2 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuSCN-0.3.
[0090] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 1.65 g of KCl and 1.35 g of LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 650 °C for 1 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-f.
[0091] Example 12
[0092] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0093] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were added to 200 mL of ultrapure water, and then 1.5 mmol of CuSO4 was added. The mixture was stirred in a 50°C water bath for 6 h, cooled, filtered, and vacuum dried to obtain a copper-loaded supramolecular precursor.
[0094] (2) Primary thermal polymerization: Pour 2 g of the copper-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tubular furnace, heat at a rate of 5 °C / min in a N2 atmosphere, and maintain at 530 °C for 6 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained.
[0095] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst, 0.15 g of LiCl, and 0.15 g of NaCl, mix well and pour into a 50 mL crucible. In a N2 atmosphere, heat at a rate of 5 °C / min and maintain at 500 °C for 5 h. The obtained product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, recorded as CuSCCN-g.
[0096] Embodiment 13
[0097] A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single-atom catalyst, characterized in that it comprises the following steps:
[0098] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were added to 200 mL of ultrapure water, and then 1.8 mmol of Cu(CH3COO)2 was added. The mixture was stirred in a 60°C water bath for 4 h, cooled, filtered, and vacuum dried to obtain a copper-loaded supramolecular precursor.
[0099] (2) Primary thermal polymerization: Pour 2 g of the copper-loaded supramolecular precursor into a 50 mL crucible, place the crucible in a tube furnace, heat at a rate of 5 °C / min in a N2 atmosphere, and maintain at 580 °C for 4 h. After cooling to room temperature, a Cu / S co-doped low-crystalline carbon nitride catalyst was obtained.
[0100] (3) Secondary thermal polymerization: Weigh 0.3 g of Cu / S co-doped low-crystalline carbon nitride catalyst and 6 g of KCl, mix well and pour into a 50 mL crucible. In a N2 atmosphere, heat at a rate of 5°C / min and maintain at 600°C for 3 h. The product is washed with ultrapure water and dried to obtain a Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst, denoted as CuSCCN-h.
[0101] Embodiment 14
[0102] This example aims to characterize the stability of the catalyst.
[0103] Taking the Cu / S in-situ co-doped high crystalline carbon nitride (CuSCCN-0.3) prepared in Example 2 as an example, its stability was investigated through a recycling experiment. The degradation experimental conditions were the same as those in Application Example 1. The catalyst of the photo-Fenton reaction was filtered and dried, and then the next cycle of degradation experiment was carried out under the same reaction conditions. This was repeated 6 times. Figure 1 As shown in the figure, after 6 cycles, the degradation rate of sulfamethoxazole in the CuSCCN-0.3 photo-Fenton system can still reach more than 90%, indicating that CuSCCN-0.3 has strong stability.
[0104] Embodiment 15
[0105] This example aims to characterize the degradation effect of the catalyst on sulfamethoxazole in the presence of different inorganic salts.
[0106] Taking the Cu / S in-situ co-doped high crystalline carbon nitride (CuSCCN-0.3) prepared in Example 2 as an example, the degradation effect of sulfamethoxazole in the presence of different inorganic salts was investigated. The degradation experimental conditions were the same as those in Application Example 1, except that 10 mM Cl - 、NO3 - 、SO4 2- 、HCO3 - 、H2PO4 - and NO3 - The results are as attached. Figure 2 The results show that Cu / S co-doped highly crystalline carbon nitride in different inorganic salts (Cl - 、NO3 - 、SO4 2- 、CO3 2- and HPO4 2- ) conditions, after 40 minutes of photo-Fenton reaction, more than 97% of sulfamethoxazole could still be degraded, showing good environmental adaptability.
[0107] Example 16
[0108] This example aims to characterize the degradation effect of the catalyst on different organic pollutants.
[0109] Taking the Cu / S in-situ co-doped high crystalline carbon nitride (CuSCCN-0.3) prepared in Example 2 as an example, its degradation effect on different organic pollutants was investigated. The degradation experimental conditions were the same as those in Application Example 1, except that the pollutant used was any one of sulfamethoxazole, sulfamethoxazole, ciprofloxacin, norfloxacin, tetracycline and oxytetracycline, under the same experimental conditions as in Application Example 1. Figure 3 As shown, after 40 minutes of photo-Fenton reaction, the degradation rates of six organic pollutants (sulfamethoxazole, sulfamethoxazole, ciprofloxacin, norfloxacin, tetracycline and oxytetracycline) by Cu / S co-doped highly crystalline carbon nitride were all higher than 99%, showing good broad-spectrum properties.
[0110] Comparative Example 1
[0111] A S-doped high-crystalline carbon nitride catalyst is prepared by the following steps:
[0112] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of thiocyanate were weighed and added into 200 mL of ultrapure water. The mixture was stirred in a water bath at 80° C. for 2 h, and then filtered and dried in a vacuum to obtain the supramolecular precursor TMCA.
[0113] (2) Primary thermal polymerization: 2 g of TMCA was weighed and poured into a 50 mL crucible. The crucible was placed in a tubular furnace. Under an Ar atmosphere, the temperature was increased at a rate of 5 °C / min and maintained at 550 °C for 2 h. After cooling to room temperature, an S-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as SCN.
[0114] (3) Secondary thermal polymerization: Weigh 0.3 g SCN, 1.65 g KCl and 1.35 g LiCl, mix well and pour into a 50 mL crucible. Under Ar conditions, heat at a rate of 5 °C / min and maintain at 550 °C for 2 h. The obtained product is washed with ultrapure water and dried to obtain an S-doped highly crystalline carbon nitride single atom catalyst, recorded as SCCN.
[0115] The obtained SCCN was subjected to a photo-Fenton reaction under the same experimental conditions as in Application Example 1.
[0116] Comparative Example 2
[0117] A Cu-doped highly crystalline carbon nitride catalyst is prepared by the following steps:
[0118] (1) Supramolecular self-assembly: 10 mmol of melamine and 10 mmol of cyanuric acid were weighed and added to 200 mL of ultrapure water, and 0.3 mmol of CuCl2 was added. After hydrothermal treatment at 180 °C for 24 h, the supramolecular precursor Cu was obtained after filtration and vacuum drying. 0.3 -MCA.
[0119] (2) Primary thermal polymerization: weigh 2 g Cu 0.3 -MCA was poured into a 50 mL crucible, and the crucible was placed in a tubular furnace. Under an Ar atmosphere, the temperature was increased at a rate of 5 °C / min and maintained at 550 °C for 2 h. After cooling to room temperature, a Cu-doped low-crystalline carbon nitride catalyst was obtained, which was recorded as CuCN-0.3.
[0120] (3) Secondary thermal polymerization: 0.3 g CuCN-0.3, 1.65 g KCl and 1.35 g LiCl were weighed, mixed and poured into a 50 mL crucible. Under Ar conditions, the temperature was increased at a rate of 5 °C / min and maintained at 550 °C for 2 h. The product was washed with ultrapure water and dried to obtain a Cu-doped highly crystalline carbon nitride single atom catalyst, recorded as CuCCN-0.3.
[0121] The obtained CuCCN-0.3 was subjected to a photo-Fenton reaction under the same experimental conditions as in Application Example 1.
[0122] Figure 4 The Cu-loaded supramolecular precursor (Cu x-TMCA, x = 0.1, 0.3, 0.5, 1 and 2) and the XRD patterns of the supramolecular precursor (TMCA) in Comparative Example 1. Figure 4 It can be seen that the XRD diffraction peaks remain consistent before and after the introduction of Cu into the supramolecular precursor, indicating that the Cu in the supramolecular precursor does not change the crystal structure of the supramolecular precursor. At the same time, after the introduction of Cu, the diffraction angle corresponding to the XRD diffraction peak of the supramolecular precursor becomes smaller, indicating that the introduction of Cu makes the unit cell size of the supramolecular precursor larger.
[0123] Figure 5 The Cu-loaded supramolecular precursor (Cu 0.3 -TMCA) and the solid UV-visible diffuse reflection absorption spectra of the supramolecular precursor (TMCA) in Comparative Example 1. Figure 5 It can be seen that the visible light absorption of the supramolecular precursor is significantly enhanced after the introduction of Cu, which is mainly attributed to the ligand metal electron transfer between Cu and trithiocyanate.
[0124] Figure 6 The Cu-loaded supramolecular precursor (Cu 0.3 -TMCA) scanning electron microscope image. Figure 6 In the figure, it can be seen that the Cu-loaded supramolecular precursors self-assemble into rod-like structures.
[0125] Figure 7 The XRD patterns of Cu / S co-doped highly crystalline carbon nitride (CuSCCN-x, x=0.1, 0.3, 0.5, 1 and 2) in Examples 1 to 5 of the present invention and S-doped highly crystalline carbon nitride (SCCN) in Comparative Example 1 are shown in FIG. Figure 7 It can be seen that with the increase of Cu loading, no diffraction peaks of Cu nanoparticles or Cu oxides appear, indicating that Cu may exist in the form of single atoms.
[0126] Figure 8 The transmission electron microscope and high-resolution transmission electron microscope images of Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention are shown in FIG. Figure 8 In a, we can see that CuSCCN-0.3 is composed of nanoparticles with a size of 20 to 30 nm. Figure 8 In b, lattice fringes with a lattice spacing of 1.05 nm can be seen, corresponding to the (001) crystal plane of polyheptazine imide, indicating the presence of highly crystalline carbon nitride.
[0127] Fig. 9 The spherical aberration corrected transmission electron microscope image and the corresponding element scanning image of Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention. Fig. 9From the ae, we can see that elements such as C, N, Cu / S are evenly distributed on the surface of the material, confirming the successful doping of Cu / S. Fig. 9 f, monodispersed bright white spots can be clearly seen, indicating the existence of single Cu atoms.
[0128] Fig.10 The performance curves of photo-Fenton degradation of sulfamethoxazole by Cu / S co-doped highly crystalline carbon nitride (CuSCCN-x, x=0.1, 0.3, 0.5, 1 and 2) in Examples 1 to 5 of the present invention, S-doped highly crystalline carbon nitride (SCCN) in Comparative Example 1 and Cu-doped highly crystalline carbon nitride (CuCCN-0.3) in Comparative Example 2 are shown. Fig.10 It can be seen that after 40 minutes of photo-Fenton reaction, the S-doped and Cu-doped highly crystalline carbon nitride in Comparative Example 1 and Comparative Example 2 degraded about 15% and 63% of sulfamethoxazole, respectively, while the photo-Fenton activity of Cu / S co-doped highly crystalline carbon nitride was much higher than that of S-doped and Cu-doped highly crystalline carbon nitride alone, indicating that S and Cu co-doping can simultaneously improve the photo-Fenton activity of crystalline carbon nitride.
[0129] Fig.11 The kinetic diagram of the photo-Fenton degradation of sulfamethoxazole by Cu / S co-doped highly crystalline carbon nitride (CuSCCN-0.3) in Example 2 of the present invention and Examples 6 to 13 (CuSCCN-a to h). Fig.11 It can be seen that the Cu / S co-doped highly crystalline carbon nitride prepared under different conditions all show excellent photo-Fenton activity.
Claims
1. A method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst, characterized in that: The following steps are involved: Step 1, mixing melamine, thiocyanate and copper salt in water and heating, cooling, filtering and drying to obtain a copper-loaded supramolecular precursor; Step 2, subjecting the copper-loaded supramolecular precursor to a thermal polymerization reaction under protective gas conditions to obtain Cu / S in-situ co-doped low-crystalline carbon nitride; Step three, after mixing the Cu / S in-situ co-doped low-crystalline carbon nitride and the molten salt, a secondary thermal polymerization reaction is carried out under protective gas conditions. After washing with water, filtering and drying, the Cu / S in-situ co-doped high-crystalline carbon nitride single atom catalyst can be obtained.
2. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In the step 1, the molar ratio of melamine, thiocyanuric acid and copper salt is 100:100:1-20.
3. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In step 1, the copper salt is one or more of CuCl2, CuSO4, Cu(NO3)2, and Cu(CH3COO)2.
4. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In the step 1, the heating temperature is 30-100° C. and the heating time is 2-8 hours.
5. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In the step 2, the temperature of the first thermal polymerization reaction is 500-600° C., and the time of the first thermal polymerization reaction is 1-8 hours.
6. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In the step 3, the molten salt is one or more of KCl, LiCl, and NaCl.
7. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In the step three, the mass ratio of Cu / S co-doped low-crystalline carbon nitride to molten salt is 1:1-20.
8. The method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 1, characterized in that: In the step 3, the temperature of the secondary thermal polymerization reaction is 450-650° C., and the time of the secondary thermal polymerization reaction is 1-6 hours.
9. The Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst obtained by the method for preparing a Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to any one of claims 1 to 8, characterized in that: The invention comprises the following substances in mass percentage: 0.09wt% to 0.32wt% of S, 0.1wt% to 10wt% of Cu, and the rest of carbon nitride; the carbon nitride is polyheptazine imide, the Cu is doped in the pores of the carbon nitride in the form of single atoms, and the S is located on the skeleton of the carbon nitride in the form of substitution doping.
10. Use of the Cu / S in-situ co-doped highly crystalline carbon nitride single atom catalyst according to claim 9 in photo-Fenton degradation of sulfamethoxazole, sulfamethoxazole, ciprofloxacin, norfloxacin, tetracycline and oxytetracycline in wastewater.
Citation Information
Patent Citations
A phosphorus- and bismuth-co-doped porous graphitic carbon nitride photocatalyst and its applications
CN109772423B
Preparation of a non-metal-doped substrate-supported metal single-atom catalyst
CN115970731B
An easily separable nickel-boron-doped carbon nitride catalyst and preparation method thereof
CN116328814B
Preparation method of sulfur-doped carbon nitride nanosheets and product and application of sulfur-doped carbon nitride nanosheets
CN110064429A
Sulfur-doped crystal carbon nitride for photocatalytic decomposition of water to produce hydrogen and preparation method and application thereof
CN112473713A
Cited By
Preparation method of cobalt modified polyheptazinyl imide and application of cobalt modified polyheptazinyl imide in rhodamine B photosensitization detection of paracetamol
CN120665286A