Preparation method and process of Fe-Mn-MOF-74 catalyst for CO-SCR denitration under medium and low temperature oxygen-enriched conditions

CN118988408APending Publication Date: 2024-11-22INNER MONGOLIA UNIVERSITY

Patent Information

Application Number
CN202411163408.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22

Smart Images

  • Figure CN118988408A_ABST
    Figure CN118988408A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and a process of a Fe-Mn-MOF-74 catalyst for CO-SCR (Selective Catalytic Reduction) denitration under a medium and low temperature oxygen-enriched condition. The Fe-Mn-MOF-74 material with high specific surface area (about 447 m / g) and efficient unsaturated bimetallic active sites is prepared by regulating and controlling the metal molar ratio of Fe to Mn and adopting a one-step hydrothermal synthesis method on the premise of ensuring that the total metal molar mass is not changed. The material shows a unique and regular rodlike porous structure, good crystallinity and uniform pore distribution. The Fe-Mn-MOF-74 catalyst has efficient NOx removal capacity, the denitration efficiency reaches up to 100% within the temperature range of 200-250 DEG C, and the denitration efficiency can still be kept at 70%-90% even under the 2-6 vol% oxygen-enriched condition. The Fe-Mn-MOF-74 catalyst prepared by the method disclosed by the invention is low in cost and easy for large-scale production, and a new thought and an efficient solution are provided for a CO-SCR denitration technology under a medium-low temperature oxygen-enriched condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial flue gas denitration catalyst preparation, and particularly to a method and process for preparing a Fe-Mn-MOF-74 catalyst for CO-SCR denitration under medium-low temperature and oxygen-rich conditions. Background Art

[0002] Nitrogen oxides (NO x ) is one of the main air pollutants emitted from industrial production and transportation, causing serious harm to human health and the ecological environment. Selective catalytic reduction (SCR) technology is a technology to remove NO x The NH3-SCR technology using ammonia (NH3) as a reducing agent has been widely used in industrial flue gas denitrification. However, the NH3-SCR technology has disadvantages such as high economic cost, ammonia leakage, equipment corrosion, and is not suitable for low-temperature flue gas (actual temperature below 300 °C). Therefore, the CO-SCR technology using carbon monoxide (CO) as a reducing agent has become a promising alternative.

[0003] In recent years, CO-SCR technology has received extensive attention and research. Studies have shown that precious metal catalysts (such as Pt, Pd, Ir, etc.) show high activity in CO-SCR, but have the following disadvantages: (1) High economic cost: Precious metal resources are scarce and expensive, which leads to high catalyst costs and limits their large-scale application; (2) Poor antioxidant capacity: Industrial flue gas contains O2, which will react with precious metal catalysts, causing catalyst poisoning and deactivation; (3) Poor stability and reusability: Precious metal catalysts are easily oxidized under high temperature and oxygen-rich conditions, resulting in decreased activity. In addition, the loading amount of precious metal catalysts is low, making it difficult to achieve large-scale production, and they are easily lost during the reaction, resulting in poor catalyst reusability.

[0004] In order to overcome the above shortcomings, researchers have explored the application of non-precious metal catalysts in CO-SCR, such as copper-based catalysts, cobalt-based catalysts, etc. However, the catalytic activity of these catalysts under medium and low temperature oxygen-rich conditions is still not high, which limits their application. In view of the above problems existing in the prior art, it is of great significance to develop a non-precious metal CO-SCR catalyst with high activity and stability under medium and low temperature oxygen-rich conditions.

[0005] The Fe-Mn-MOF-74 catalyst provided by the present invention realizes uniform dispersion and exposure of metal active sites through its unique metal organic framework structure, has good oxygen reduction performance, and exhibits excellent CO-SCR catalytic activity under medium and low temperature oxygen-rich conditions. The catalyst has the following advantages: (1) Low cost: Fe and Mn are common metal elements with abundant resources and low prices, which is conducive to reducing catalyst costs; (2) Strong anti-oxidation ability: The MOF structure has good stability and can effectively resist the influence of O2 and extend the service life of the catalyst; (3) High activity at medium and low temperatures: The MOF structure can effectively improve the interaction and exposure between metal active sites, enhancing the activity of the catalyst under medium and low temperature conditions; (4) Easy to prepare: MOF materials can be synthesized in one step by hydrothermal method and can be easily produced on a large scale.

[0006] The Fe-Mn-MOF-74 catalyst prepared by the present invention provides a new idea and solution for the application of CO-SCR technology under medium and low temperature oxygen-rich conditions, and has important theoretical significance and application value. Summary of the invention

[0007] In view of the defects existing in the prior art, the present invention relates to a Fe-Mn-MOF-74 catalyst for CO-SCR denitration under medium-low temperature oxygen-rich conditions and a preparation method and application thereof, and in particular to a Fe-Mn-MOF-74 catalyst synthesized by a one-step hydrothermal method, which has excellent denitration activity under medium-low temperature oxygen-rich conditions and is suitable for industrial source flue gas emission of NO x Efficient removal.

[0008] The technical solution adopted by the present invention is: Step 1: Under the premise that the total metal molar mass is 1.54 mmol, 0.272-0.815 g of FeCl2·4H2O and 0.824-0.275 g of MnCl2·4H2O, where the metal molar ratios of metal Fe and Mn are (0.25-0.26: 0.74-0.75, 0.5-0.57: 0.43-0.5, 0.71-0.75: 0.25-0.29 mmol) and 1.68 mmol of 2,5-dihydroxyterephthalic acid are dissolved in 150 mL of a solution with a volume ratio of N,N-dimethylformamide (DMF): ethanol: water = 15:1:1, and stirred evenly with a glass rod and ultrasonically mixed for 30 min. The resulting solution is placed in multiple 80 mL high-pressure reactors and placed in a forced air drying oven for reaction at 120-135 ° C for 24 h.

[0009] Step 2: Place the solution obtained after the reaction in step 1 into multiple 75 mL centrifuge tubes, and place them in a high-speed centrifuge at a speed of 8000-12000 r / min to separate the products. In this process, use DMF and ethanol solutions to wash the catalyst three times each. Place the product after centrifugation into a beaker, immerse it in 50-60 mL of methanol solution, and stir it with a magnetic stirrer for 30 minutes. After stirring evenly, seal the beaker with a sealing film and place it in a fume hood. The immersion and replacement time is 3 days, and the solution is replaced every 24 hours during this period.

[0010] Step 3: Pour off the supernatant from the solution obtained in step 2, leaving the precipitate, and place it in a vacuum drying oven at 65-80 °C for constant temperature drying for 8-12 h. After drying, grind the sample into a 40-60 mesh powder, place the sample in a quartz boat, and activate it in a tube furnace at an activation temperature range of 200-250 °C and a N2 atmosphere of 25mL / min. The activated Fe-Mn-MOF-74 catalyst is obtained and loaded into a sample tube for standby use.

[0011] The prepared Fe-Mn-MOF-74 catalyst was used for CO-SCR denitrification performance evaluation: 200 mg of catalyst (40-60 mesh) was placed in a fixed bed quartz reactor and pretreated at 100 °C for 0.5 h in an Ar atmosphere to remove moisture and impurities. The test temperature range was then 50-250 °C. The laboratory simulated reaction conditions were: [NO] 500 ppm, [CO] 1000 ppm, 2-6 vol% O2 (when used), and Ar as the balance gas. The total flow rate was controlled at 150 mL min -1 , gas space velocity GHSV = 30000 h -1 The corresponding gas concentrations are detected by flue gas analyzer Testo 350, and the tail gas is treated with alkali solution.

[0012] Compared with the prior art, the present invention has the following beneficial effects: (1) Fe-Mn-MOF-74 catalyst has excellent medium-low temperature denitrification activity and antioxidant properties, and is suitable for industrial source flue gas emission of NO under medium-low temperature oxygen-rich conditions x Efficient removal of (2) The preparation method of Fe-Mn-MOF-74 catalyst is simple, low-cost, and easy to industrialize; (3) The Fe-Mn-MOF-74 catalyst has good stability and reusability, long service life, and has the potential for practical application. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for describing the embodiments.

[0014] Figure 1 SEM images of the prepared catalyst Fe1-Mn1-MOF-74, with magnifications of (a, c) 5 μm and (b, d) 1 μm. The scanning results show that the catalyst surface presents a unique and regular polyhedral rod-like structure, and the overall morphology is like a "twisted flower" with a small particle size.

[0015] Figure 2 (a) is the XRD pattern of the prepared series of Fe-Mn-MOF-74 catalysts. Figure 2 (b) XRD spectrum of Fe1-Mn1-MOF-74 catalyst before and after the SCR reaction and oxygen-rich conditions; the results show that the bimetallic MOF-74 catalyst was successfully synthesized, and the catalyst structure of the catalyst with a metal molar ratio of Fe:Mn=1:1 remained unchanged before and after the reaction.

[0016] Figure 3 Thermogravimetric diagrams of the prepared series of Fe-Mn-MOF-74 catalysts; the test results show that when the temperature does not exceed 250°C, the catalyst maintains the metal skeleton structure unique to MOFs materials, and as the temperature increases, the volatilization of water molecules and excess solvent on the surface and inside of the catalyst is beneficial to improving the catalytic activity.

[0017] Figure 4 (a) is the test curve of CO-SCR denitrification activity of the prepared Fe-Mn-MOF-74 catalyst under different reaction conditions. Figure 4 (b) is the NO conversion rate of Fe1-Mn1-MOF-74 catalyst under oxygen-rich conditions. The results show that the introduction of Fe improves the denitrification activity of the catalyst, and the highest NO conversion rate can reach 100%. Even under oxygen-rich conditions of 2-6 vol% O2, Fe1-Mn1-MOF-74 catalyst can still maintain a NO conversion rate of 70%-90%.

[0018] Figure 5 Phase structure test diagram for the preparation of Fe-Mn-MOF-74 catalyst: (a) FTIR spectrum, (b) Raman spectrum.

[0019] Figure 6 The stability test diagram of Fe1-Mn1-MOF-74 catalyst under different reaction conditions. The results show that the NO conversion rate of the catalyst has no downward trend after 10 hours of continuous reaction under anaerobic conditions, and the NO removal rate is still above 96% under 2-6 vol% O2 oxygen-rich conditions.

[0020] Figure 7 The reusability test diagram of the Fe1-Mn1-MOF-74 catalyst under oxygen-free and 2-6 vol% O2-enriched conditions was prepared. The results showed that after 6 cycles of testing, the NO conversion rate of the catalyst only decreased by 0.5-2%, indicating that the catalyst can be recycled multiple times and has excellent cyclic stability.

[0021] Figure 8 The N2 selectivity test diagram of the Fe1-Mn1-MOF-74 catalyst under oxygen-free and 2-6 vol% O2-enriched conditions at the optimal reaction temperature of 250 °C was prepared. The results show that the N2 selectivity of the catalyst remains above 96%, maintaining a high value.

[0022] Fig. 9 N2 adsorption and desorption and pore size distribution diagram of the Fe-Mn-MOF-74 catalyst series. Fig. 9 (a) is the catalyst specific surface area test, Fig. 9 (b) is the catalyst pore structure test. The results show that the specific surface area of ​​Fe1-Mn3-MOF-74 is 383.354 m 2 ·g -1 The specific surface area of ​​Fe1-Mn1-MOF-74 is 447.525 m 2 ·g -1 The specific surface area of ​​Fe3-Mn1-MOF-74 is 426.557 m 2 ·g -1 The average pore size is 5.3-6.8 nm, and the catalyst has a micro-mesoporous structure dominated by mesopores.

[0023] Fig.10 In-situ infrared spectrum of the Fe1-Mn1-MOF-74 catalyst prepared at the optimal reaction temperature of 250 °C for 1 h. Fig.10 (a) is the catalyst co-adsorbing NO+CO, Fig.10 (b) is the catalyst that co-adsorbs NO+CO+2%O2, Fig.10 (c) is the catalyst that co-adsorbs NO+CO+4%O2, Fig.10 (d) The catalyst co-adsorbs NO+CO+6%O2. The results show that there is adsorption and conversion of CO and NO gases on the catalyst surface, and the presence of -1 At 2335 and 2360 cm -1 Under oxygen-rich conditions, the adsorbed NO is converted to highly oxidized nitrate, and overlapping peaks of carbonyl and N2O4 species appear (1747 cm -1 ), chelated bidentate nitrate (1480 cm -1), key intermediate Fe 2+ -(NO)2 2- The NN vibration of the substance (1260 cm -1 )New absorption peak.

[0024] Fig.11 NO-TPD test diagram for the preparation of Fe1-Mn1-MOF-74 catalyst. The results show that after the introduction of Fe, the catalyst has more types of acid centers, more desorption peaks with larger peak areas, and abundant surface acid sites and acid strength.

[0025] Fig.12 XPS test diagram of the prepared Fe1-Mn1-MOF-74 catalyst, (a) overall spectrum, (b) 2p orbital of Mn, (c) 2p orbital of Fe, and (d) 1s orbital of O. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with specific embodiments. Example 1

[0027] Preparation of Mn-MOF-74: MnCl2·4H2O (5.55 mmol) and 2,5-dihydroxyterephthalic acid (1.68 mmol) were dissolved in 150 mL of a solution with a volume ratio of N,N-dimethylformamide (DMF): ethanol: water = 15:1:1. A glass rod was used to stir evenly during the dissolution process, and ultrasonic mixing was performed for 30 min. The solution was then placed in multiple 80 mL high-pressure reactors and placed in an oven set to 135 °C for 24 h. After the reaction, the product was separated by a high-speed centrifuge (8000 r / min). In this process, the catalyst was washed three times with DMF and ethanol respectively. The obtained product was placed in a beaker and immersed in an appropriate amount of methanol for 3 days. The solution was replaced every 24 h, and then placed in a vacuum drying oven at 65 °C for overnight drying. The dried sample was ground into powder (40-60 mesh) and placed in a quartz boat, and activated in a tube furnace at 250 °C in a N2 atmosphere (25 mL / min) for 6 h to obtain Mn-MOF-74. This material was used as a control material for the bimetallic composite catalytic material. Example 2

[0028] Preparation of Fe1-Mn3-MOF-74: 0.272 g FeCl2·4H2O, 0.824 g MnCl2·4H2O and 0.333 g 2,5-dihydroxyterephthalic acid were dissolved in 150 mL mixed solvent (DMF: ethanol: water = 15:1:1), stirred evenly with a glass rod, ultrasonically mixed for 30 min, and placed in an 80 mL autoclave for reaction at 120-135 °C for 24 h. Subsequently, the reaction solution was centrifuged and washed three times with DMF and ethanol, and the precipitate was soaked in 50-60 mL methanol and allowed to stand for 3 days, during which the methanol was replaced every 24 h. Finally, the precipitate was dried and ground into 40-60 mesh, and activated in N2 atmosphere (25 mL / min) at 200-250 °C to obtain Fe1-Mn3-MOF-74, in which the preset molar ratio of Fe:Mn=0.25-0.26:0.74-0.75 mmol. Example 3

[0029] Preparation of Fe1-Mn1-MOF-74: 0.544 g FeCl2·4H2O, 0.548 g MnCl2·4H2O and 0.333 g 2,5-dihydroxyterephthalic acid were dissolved in 150 mL mixed solvent (DMF: ethanol: water = 15:1:1), stirred evenly with a glass rod, and then ultrasonically mixed for 30 min, placed in an 80 mL high-pressure reactor at 120-135 ° C for 24 h. Subsequently, the reaction solution was centrifuged and washed three times with DMF and ethanol, and the precipitate was soaked in 50-60 mL methanol and allowed to stand for 3 days, during which the methanol was replaced every 24 h. Finally, the precipitate was dried and ground into 40-60 mesh, and activated in N2 atmosphere (25 mL / min) at 200-250 °C to obtain Fe1-Mn1-MOF-74, in which the preset molar ratio of Fe:Mn=0.5-0.57:0.43-0.5. Example 4

[0030] Preparation of Fe3-Mn1-MOF-74: 0.815 g FeCl2·4H2O, 0.275 g MnCl2·4H2O and 0.333 g 2,5-dihydroxyterephthalic acid were dissolved in 150 mL mixed solvent (DMF: ethanol: water = 15:1:1), stirred evenly with a glass rod, and then ultrasonically mixed for 30 min, placed in an 80 mL autoclave and reacted at 120-135 ° C for 24 h. Subsequently, the reaction solution was centrifuged and washed three times with DMF and ethanol, and the precipitate was soaked in 50-60 mL methanol and allowed to stand for 3 days, during which the methanol was replaced every 24 h. Finally, the precipitate was dried and ground into 40-60 mesh, and activated in N2 atmosphere (25 mL / min) at 200-250 °C to obtain Fe3-Mn1-MOF-74, in which the preset molar ratio of Fe:Mn=0.71-0.75:0.25-0.29 mmol. Example 5

[0031] Evaluation of catalyst denitrification activity: The test for evaluating the reaction activity of the catalyst was carried out in a fixed bed quartz reactor with an inner diameter of 7 mm and a length of 450 mm. 200 mg (40-60 mesh) of catalyst was placed in the center of the quartz tube and fixed with quartz wool to fill the gap. Before the test, the catalyst was pretreated for 0.5 h at a temperature of 100 ° C and an Ar gas atmosphere (25 mL / min) to remove moisture and impurities. Subsequently, the reactor was cooled to the target temperature and the denitrification activity evaluation test was carried out. The laboratory simulated flue gas condition parameters were set as: [NO] 500 ppm, [CO] 1000 ppm, 2-6 vol% O2 (4000-12000 ppm) When used, Ar was used as a balance gas, the total flow rate was 150 mL / min, and the gas space velocity GHSV was 30000h -1 The NO and N2 selectivities are calculated by the following equations (1)-(2): NO\, Conversion(\% )=\frac {{[NO]}_{in}-{[NO]}_{out}} {{[NO]}_{in}}\times 100\% {N}_{2}\, Selectivity(\% )=[1-\frac {2[{N}_{2}O]} {{[NO]}_{in}-{[NO]}_{out}]}]\times 100\% The N2 selectivity is measured by collecting the exhaust gas after the CO-SCR reaction at different reaction temperatures, storing it in an air bag, and then extracting a certain volume of gas with a needle, injecting it into a gas chromatograph with a N2O column, and taking the average value of three measurements.

[0032] The denitrification activity of the prepared series of catalysts was investigated in the temperature range of 50-250 °C. The specific results are as follows: (1) For the Mn-MOF-74 catalyst, the NO conversion rate gradually increased with the increase of temperature, reaching a maximum of 57.89%. Under 2-6 vol% O2-enriched conditions, the NO conversion rate was only 15.45%-45.82%; (2) For Fe1-Mn3-MOF-74 catalyst, the NO conversion rate exceeded 70% at 200 °C and reached 76.25% at 250 °C; (3) For Fe1-Mn1-MOF-74 catalyst, under oxygen-free conditions, the NO conversion rate exceeds 80% at 200 °C, and the NO conversion rate is close to 100% at 250 °C. Under 2-6 vol% O2-enriched conditions, the catalyst can still maintain a NO removal rate of 70%-90%. In addition, the selectivity of N2 generation remains stable at 98% under oxygen-free conditions, and the N2 selectivity under oxygen-enriched conditions is 96.60%-97.59%; (4) For Fe3-Mn1-MOF-74 catalyst, the NO conversion rate exceeded 70% at 200 °C and reached 80.94% at 250 °C.

[0033] The present invention successfully prepared a CO-SCR catalyst, which exhibited a NO conversion rate of up to 100% in the temperature range of 200-250 ℃, and could still maintain a NO conversion rate of 70%-90% under oxygen-rich conditions of 2-6 vol% O2. With its excellent medium and low temperature denitrification performance and anti-oxidation performance, the catalyst has significant industrial application potential and provides new ideas and references for flue gas denitrification technology.

Claims

1. A method and process for preparing Fe-Mn-MOF-74 catalyst for CO-SCR denitration under medium and low temperature oxygen-rich conditions, comprising the following steps: Step 1: Dissolve MnCl2·4H2O, FeCl2·4H2O and 2,5-dihydroxyterephthalic acid in a certain proportion in a solution with a volume ratio of N,N-dimethylformamide (DMF): ethanol: water = 15:1:1, stir evenly and mix by ultrasonic. Place the obtained solution in multiple high-pressure reactors and place them in a constant temperature forced air drying oven for reaction; Step 2: The solution obtained after the reaction in step 1 is separated by a high-speed centrifuge, and the catalyst is washed three times with DMF and ethanol solutions respectively during this process. The product obtained after centrifugation is placed in a beaker, immersed in an appropriate amount of methanol solution, and stirred evenly with a magnetic stirrer. The beaker is then sealed with a sealing film and placed in a fume hood, and the methanol solution is replaced at specific intervals; Step 3: Pour off the supernatant of the solution obtained in step 2, leaving the precipitate, and place it in a vacuum drying oven to dry overnight. After drying, grind the sample into powder and place it in a quartz boat, and activate it in a tube furnace at a certain activation temperature and N2 atmosphere. The activated Fe-Mn-MOF-74 catalyst is obtained and loaded into a sample tube for standby use.

2. According to claim 1, it is characterized in that: In the step 1, under the premise that the total metal molar mass is 0.305 g (1.54 mmol), the dosages of MnCl2·4H2O and FeCl2·4H2O are respectively FeCl2·4H2O (0.272-0.815 g, 1.37-4.10 mmol) and MnCl2·4H2O (0.824-0.275 g, 4.16-1.39 mmol), wherein the molar ratio of the metals is Fe:Mn=(0.25-0.26:0.74-0.75, 0.5-0.57:0.43-0.5, 0.71-0.75:0.25-0.29), and the dosage of 2,5-dihydroxyterephthalic acid is 0.333 g (1.68 mmol); the total volume of the mixed solvent of N,N-dimethylformamide (DMF): ethanol: water = 15:1:1 is 150 mL; the ultrasonic mixing time is 30 min; the volume of the lining of the high-pressure reactor is 80 mL; the temperature of the blast drying oven is set to 120-135 ° C, and the reaction time is 24 h.

3. According to claim 1, it is characterized in that: In step 2, the centrifuge speed used is 8000-12000 r / min; the stirring time of the magnetic stirrer is 30 min; the volume of the methanol solution used for immersion is 50-60 mL, the immersion replacement time is 3 days, and the solution is replaced every 24 hours.

4. According to claim 1, it is characterized in that: In step 3, the temperature of the vacuum drying oven is set to 65-80°C, the drying time is 8-12 h, the sample powder size is 40-60 mesh, the activation temperature is 200-250°C, and the N2 flow rate is 25 mL / min.

5. Application of the Fe-Mn-MOF-74 catalyst prepared by the preparation method according to any one of claims 1 to 4 in CO-SCR, characterized in that: Applicable to industrial source flue gas emission NO x Efficient removal.

Citation Information

Patent Citations

  • Sulfur dioxide resistant type low temperature ferromanganese oxide denitration catalyst and preparation method thereof

    CN104437537A

  • Preparation method of Mn-based rodlike microtopography composite oxide low-temperature denitrification catalyst

    CN104624199A

  • Synthesis method and application of MOF-74-NiCo material

    CN109701657A

  • Low-temperature denitration catalyst based on metal organic framework structure and preparation method thereof

    CN110961157A

  • CO-SCR denitration catalyst as well as preparation method and application thereof

    CN111229212A

Cited By

  • Photocatalytic material with baseball-shaped structure as well as preparation method and application of photocatalytic material

    CN121244292A

  • A photocatalytic material with a baseball-like structure, and a preparation method and application thereof

    CN121244292B