Method for enhancing compressive strength of hollow microspheres

The tiny cracks and defects of hollow microbeads are removed through water-resistant isostatic equipment, which significantly improves its compressive strength, solves the problem of low compressive strength, expands the application field and improves the performance of composite materials.

CN118988515AActive Publication Date: 2024-11-22CNBM RESEARCH INSTITUTE FOR ADVANCED GLASS MATERIALS GROUP CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411010353.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-22
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The compressive strength of hollow microbeads is low, resulting in easy breakage in ultra-high pressure and low density applications, limiting their performance in composite materials, especially in poor addition effects in solid buoyancy materials.

Method used

The micro cracks in hollow microbeads are pre-removed and defects such as eccentricity and multi-cavity generated during the production process are used to improve the compressive strength through the boosting and holding process, and combined with gravity bleaching and pressure detection, we can obtain Ultra-high pressure hollow microbeads.

Benefits of technology

The overall strength of hollow microbeads has been significantly improved, the application areas have been expanded, and the performance of composite materials as additives has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988515A_ABST
    Figure CN118988515A_ABST
Patent Text Reader

Abstract

The invention discloses a method for enhancing compressive strength of hollow microspheres, and relates to the technical field of hollow microsphere treatment. In the manufacturing process of traditional hollow microspheres, due to the fact that the interiors of the hollow microspheres have nonuniformity, especially vacancies are gathered due to thermal diffusion, gaps are formed, and then crack cores are formed under the action of stress. The crack nuclei diffuse to the surface of the glass and gather and develop into microcracks. In addition, the structure of the glass surface also has influence on generation of microcracks. Under the ultrahigh pressure condition, the tiny micro cracks directly limit the upper limit of the strength of the hollow microspheres, and the water-resistant isostatic pressing equipment is used for removing the hollow microspheres which have the tiny cracks and are low in compressive strength, such as eccentricity, multiple cavities and the like generated in other production processes in advance, so that the strength of the rest integral hollow microsphere product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hollow microsphere processing, in particular to a method for enhancing the compressive strength of hollow microspheres. Background Art

[0002] Hollow microspheres are hollow, tiny spherical materials containing inert gas, with a density of 0.1-0.7g / cm 3 , the particle size range is generally 5-200μm. It is a hollow particle with unique and stable properties. Due to its low density, low thermal conductivity, low dielectric constant, and chemical corrosion resistance, it is widely used in military, civilian and other high-tech fields such as solid buoyancy materials, petrochemicals, emulsion explosives, thermal insulation and fireproof materials, invisible silencing materials, advanced insulation materials, chemical product additives, and low-density ablative materials. However, with the continuous development of science and technology and the continuous development of new application fields, the performance requirements of hollow microspheres are getting higher and higher, especially the compressive strength performance. For example, when added to polymer materials to prepare low-density materials, especially solid buoyancy materials, the hollow microspheres are easy to break due to their relatively low compressive strength, resulting in the addition effect is not obvious and the effect is not strong; currently, it is difficult for hollow microspheres to meet their ultra-high pressure and low density requirements in commercial use, so the preparation of an ultra-high pressure hollow microsphere will help expand the application field of hollow microspheres on the one hand, and on the other hand, it will help improve the overall performance of composite materials with hollow microspheres as additives. The study found that due to the inhomogeneity inside the glass beads, especially the vacancies gathered due to thermal diffusion, forming voids, and then forming crack nuclei under the action of stress. The crack nuclei diffused to the glass surface, gathered and developed into microcracks. In addition, the structure of the glass surface also affects the formation of microcracks. The Si-O-R+ on the glass surface reacts with H2O in the air to generate SiOH groups.

[0003] Si-O-R++H2O=SiOH+ROH

[0004] Due to H + The size is R + Due to the small size of the glass beads, tensile stress on the surface of the glass beads can easily cause surface microcracks. The microcracks on the surface of the glass beads are very small, and so far, there is no way to observe them directly. Glass is a typical brittle material with great brittleness, so it is also very sensitive to tiny defects. The strength of the glass beads is determined by the existence of surface microcracks and the force expansion of small cracks.

[0005] Under ultra-high pressure conditions, these tiny microcracks directly limit the upper limit of the strength of the hollow microspheres. Therefore, it is feasible to use a water-resistant isostatic pressing equipment to pre-remove these hollow glass microspheres with tiny cracks and other eccentric, multi-cavity and other low compressive strength generated during the production process, thereby improving the strength of the remaining overall hollow microsphere products. Summary of the invention

[0006] The purpose of the present invention is to provide a method for enhancing the compressive strength of hollow microspheres, aiming to improve the strength of existing hollow microspheres.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for enhancing the compressive strength of hollow microspheres uses water-resistant isostatic pressing equipment to pre-remove hollow microspheres with microcracks and other low compressive strength such as eccentricity, multi-cavity, etc. generated during the production process, thereby obtaining ultra-high pressure hollow microspheres.

[0009] Specifically, the following steps are included:

[0010] 1. Before pressing, put the hollow microbead powder in the filter cloth bag and soak it in water to prevent instantaneous explosion under pressure during pressing.

[0011] 2. Use water-resistant isostatic pressing equipment to increase the pressure at a rate of 1-30Psi / second. Maintain the pressure for 2 minutes at 100-1500Psi. Continue to increase the pressure if there is no problem. Maintain the pressure for 30-60 minutes to the maximum pressure and then release the pressure.

[0012] 3. The hollow microbeads after being pressed are subjected to gravity floatation to remove broken glass microbeads and select hollow microbeads floating on the water surface.

[0013] 4. Use pressure testing equipment to test the recovered hollow microspheres, test their compressive strength values, and obtain ultra-high pressure hollow microspheres.

[0014] Furthermore, the specification of the filter cloth bag in step 1 is 200-1000 mesh.

[0015] Furthermore, the soaking time in step 1 is 12-24 hours.

[0016] Furthermore, since the density of hollow microspheres is different, which represents different standard compressive strengths, the maximum pressure in step 2 is determined according to the density of the hollow microspheres.

[0017] It should be further explained that the above method is also applicable to the treatment of hollow ceramic balls, inorganic hollow balls and other products.

[0018] Beneficial effects of the present invention:

[0019] The present invention utilizes a water-resistant isostatic pressing device to pre-remove hollow microspheres with low compressive strength due to micro cracks and other eccentric, multi-cavity and other factors generated in the production process from the hollow microsphere raw powder, thereby improving the strength of the remaining integral hollow microsphere product. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described below in conjunction with the accompanying drawings.

[0021] Figure 1 It is a flow chart of the present invention.

[0022] Figure 2 Comparison of hollow microspheres before and after water isostatic pressing: (a) eccentric hollow microspheres; (b) microcracked and broken hollow microspheres; (c) hollow microspheres with uneven wall thickness; (d) electron microscopic image of hollow microspheres before pressing; (e) electron microscopic image of hollow microspheres after pressing; (f) electron microscopic image of hollow microspheres after gravity floatation. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The following examples are all according to Figure 1 The process shown is implemented.

[0025] Example 1: H series hollow glass microspheres with a raw powder density of 0.120 g / cm3 and a standard compressive strength of 200 Psi (20% crushing rate) were selected. The powder was placed in an 800-mesh filter cloth bag and fully soaked in water for 24 hours. After being taken out and drained, the water-containing filter cloth bag was placed in a water-resistant isostatic pressing device. The pressure increase rate was set to 1 Psi / second, and the pressure was maintained for 2 minutes for every 100 Psi. Finally, the pressure was pressed to a maximum pressure of 300 Psi and maintained for 30 minutes. After pressing, the hollow microspheres floating on the surface were selected by gravity bleaching and dried. After being tested by a hollow glass microsphere (gas) pressure tester, the compressive strength reached 400 Psi (20% crushing rate).

[0026] Example 2: In the same case as above, the M series hollow glass microspheres with a raw powder density of 0.406g / cm3 and a standard compressive strength of 6,000Psi (20% crushing rate) were selected. The above method was used to increase the pressure at a rate of 5Psi / second, maintain the pressure for 2 minutes at every 1500Psi, and pressurize to a maximum pressure of 8,800Psi. After pressing, the powder was gravity floated and dried again. After testing by a hollow glass microsphere (gas) pressure tester, the compressive strength reached 10,500Psi (20% crushing rate).

[0027] Example 3: The density of H series hollow glass microspheres original powder is 0.650g / cm3, and the standard compressive strength is 8,000Psi (20% crushing rate). The above method is used to increase the pressure at a rate of 10Psi / second, maintain the pressure for 2 minutes at each 1500Psi, and pressurize to a maximum pressure of 10,000Psi. After pressing, gravity bleaching and drying are performed again. After testing by a hollow glass microsphere (gas) pressure tester, the compressive strength reaches 12,000Psi (20% crushing rate).

[0028] like Figure 2 As shown, it is a comparison diagram of the hollow microspheres before and after water-resistant isostatic pressing in the above embodiment. It can be clearly seen from the figure that after the operation, the uniformity and integrity of the hollow microspheres are greatly improved, thereby improving the strength.

[0029] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A method for enhancing the compressive strength of hollow microspheres, It is characterized in that The following steps are involved:

1. Before pressing, put the hollow microbead powder in the filter cloth bag and soak it in water; 2. Use water-resistant isostatic pressing equipment to increase the pressure at a rate of 1-30Psi / second, maintain the pressure for 2 minutes at 100-1500Psi, and continue to increase the pressure if there is no problem. Maintain the pressure for 30-60 minutes to the highest pressure and then release the pressure; 3. The hollow microbeads after being pressed are subjected to gravity floatation to remove broken glass microbeads and select hollow microbeads floating on the water surface; 4. Use pressure testing equipment to test the recovered hollow microspheres, test their compressive strength values, and obtain ultra-high pressure hollow microspheres.

2. A method for enhancing the compressive strength of hollow microspheres according to claim 1, It is characterized in that The specification of the filter bag in step 1 is 200-1000 mesh.

3. A method for enhancing the compressive strength of hollow microspheres according to claim 1, It is characterized in that The soaking time in step 1 is 12-24 hours.

4. A method for enhancing the compressive strength of hollow microspheres according to claim 1, It is characterized in that Since the density of hollow microspheres is different, representing different standard compressive strengths, the maximum pressure in step 2 is determined according to the density of hollow microspheres.

Citation Information

Patent Citations

  • Preparation method for preparing low-density bond cement check block for oil well by microcrystal glass beads

    CN103408263A

  • Method used for fermentation of microbial oil with low value biomass

    CN107828829A

  • Capsule for the preparation of infusion and soluble beverages

    CN109689533A

  • Microarray structure patterning process

    CN113213419A

  • Device and method for treating VOCs (Volatile Organic Compounds) by coupling micro-nano bubble catalytic oxidation and adsorption

    CN115400583A