Surface treatment method of aluminum alloy battery tray

Through degreasing, alkali corrosion, soaking and coating specific coatings, coatings with strong adhesion, corrosion resistance and waterproofness are formed, which solves the problem of poor density and durability of waterproof layers in the existing aluminum alloy surface treatment, and extends the problem of long-term stability and durability of waterproof layers. The service life of the aluminum alloy battery tray.

CN118988691AInactive Publication Date: 2024-11-22GUANGYA ALUMINUM +1

Patent Information

Application Number
CN202411027373.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing aluminum alloy surface treatment methods cannot achieve a dense waterproof layer, and the coating aging and falling off under ultraviolet light, affecting the corrosion resistance and service life of aluminum alloy.

Method used

After degreasing, alkali corrosion, polishing, soaking and drying, nano-sodium silicate, sodium molybdate, tin chloride and ammonium phosphate treatment solution, and ethylene oxide, titanium dioxide, and silicon are coated on the surface of the dried aluminum alloy. The coatings prepared by materials such as sodium acid, N,N-dimethacrylamide, boron nitride particles and ethyl cellulose form excellent network interwoven structures, enhancing waterproof and corrosion resistance.

Benefits of technology

The coating with strong adhesion, corrosion resistance and significant waterproof performance is formed, which extends the service life of the aluminum alloy battery tray and avoids the corrosion acceleration problem caused by the coating falling off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968928690000081
    Figure BDA0004968928690000081
Patent Text Reader

Abstract

The invention discloses a surface treatment method for an aluminum alloy battery tray, and belongs to the field of aluminum alloy surface treatment.The surface treatment method comprises the steps that through degreasing treatment, alkali corrosion treatment, polishing treatment, soaking treatment, drying treatment and coating treatment, components in treatment liquid are loaded on the surface of the aluminum alloy battery tray and enter holes obtained after alkali corrosion, and the corrosion resistance is promoted; besides, the paint compounded by the invention cannot have more excellent compatibility and adhesion with the soaked components, and can form excellent network interweaving in the process of forming a coating, so that the coating with remarkable waterproof performance and corrosion resistance is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum alloy surface treatment, and in particular to a surface treatment method for an aluminum alloy battery tray. Background Art

[0002] Aluminum alloy materials are widely used in automobile manufacturing, mobile phones, computers, watches, batteries and other industries due to their low density, high mechanical strength, strong corrosion resistance, and outstanding electrical and thermal conductivity. Aluminum alloys are easily recycled and are favored as green and environmentally friendly structural materials. In order to give aluminum alloys better surface corrosion resistance and other properties, the prior art forms a film layer by electroplating after sandblasting the surface of the aluminum alloy, thereby reducing the impact of the aluminum alloy on the environment and extending its service life. For example, Chinese patent number CN104805485 A discloses a surface treatment method for die-cast aluminum alloys, which relates to the field of metal surface treatment technology. The surface treatment method for die-cast aluminum alloys includes the following steps: S10, grinding the die-cast aluminum alloy; S20, sandblasting the die-cast aluminum alloy after grinding; S30, anodizing the die-cast aluminum alloy after sandblasting to form an oxide film layer on the surface of the die-cast aluminum alloy; S40, dyeing the die-cast aluminum alloy after anodizing; S50, sealing the die-cast aluminum alloy after dyeing. However, this surface treatment method cannot achieve a dense waterproof layer. In the prior art, there are also methods of spraying or coating different functional coatings on the surface of aluminum alloy to increase the surface density of aluminum alloy, thereby improving its waterproof and corrosion resistance, but there is a problem that the coating ages and falls off under the action of ultraviolet light. The fallen coating area will accelerate the corrosion of the aluminum alloy and also affect the performance of the aluminum alloy. Therefore, the present application intends to provide a surface treatment method for aluminum alloy, so that it has long-term corrosion resistance. Summary of the invention

[0003] Based on this, in order to solve the problem of poor corrosion resistance and durability of aluminum alloy surface treatment in the prior art, the present invention provides a surface treatment method for an aluminum alloy battery tray, and the specific technical solution is as follows:

[0004] A surface treatment method for an aluminum alloy battery tray, the surface treatment method comprising the following steps:

[0005] The aluminum alloy battery tray is subjected to degreasing, alkaline etching and polishing treatment to obtain an aluminum alloy battery tray with a clean surface;

[0006] The aluminum alloy battery tray with a clean surface is soaked, dried and coated;

[0007] Among them, the immersion treatment is: immersing the aluminum alloy battery tray with a clean surface in a treatment solution prepared in advance, and the treatment solution includes nano sodium silicate, sodium molybdate, tin chloride and ammonium phosphate, and the concentration of nano sodium silicate is 5g / L~8g / L, sodium molybdate is 12g / L~20g / L, tin chloride is 9g / L~13g / L and ammonium phosphate is 7g / L~10g / L.

[0008] Furthermore, the degreasing treatment is performed by adding a mixed solution of trisodium phosphate, nonylphenol polyoxyethylene ether and sodium dodecyl sulfate and heating the mixture to 45° C. to 65° C. for 20 min to 45 min.

[0009] Furthermore, the concentration of trisodium phosphate is 80 g / L to 90 g / L, the concentration of nonylphenol polyoxyethylene ether is 5 mL / L to 6 mL / L, and the concentration of sodium dodecyl sulfate is 3 g / L to 5 g / L.

[0010] Furthermore, the alkaline etching treatment uses sodium hydroxide with a concentration of 20g / L to 45g / L.

[0011] Furthermore, the temperature of the alkali etching treatment is 45° C. to 65° C., and the time is 30s to 50s.

[0012] Furthermore, the immersion treatment temperature is 60° C. to 85° C., the ultrasound-assisted frequency is 20 kHz to 50 kHz, and the time is 30 min to 50 min.

[0013] Furthermore, the drying process is carried out in a nitrogen atmosphere at a temperature of 80° C. to 110° C. and for a time of 15 min to 30 min.

[0014] Furthermore, the coating treatment is to apply a coating with a thickness of 30μm to 80μm on the surface of the dried aluminum alloy battery tray, and the coating includes the following preparation raw materials in parts by weight: 30 to 45 parts of ethylene oxide, 7 to 10 parts of titanium dioxide, 3 to 7 parts of sodium silicate, 7 to 11 parts of N,N-dimethylacrylamide, 1 to 20 parts of boron nitride particles and 2 to 7 parts of ethyl cellulose.

[0015] Furthermore, the preparation method of the coating comprises the following steps: adding ethylene oxide, titanium dioxide, sodium silicate, N,N-dimethylacrylamide, boron nitride particles and ethyl cellulose into a stirring kettle, and stirring and mixing for 30 minutes to 60 minutes to obtain the coating.

[0016] Furthermore, the average particle size of the boron nitride particles is 80 nm to 100 nm.

[0017] In the above scheme, after the aluminum alloy battery tray is immersed in water, the components in the treatment liquid are loaded on its surface and also enter into the pores after alkaline etching, which promotes corrosion resistance. In addition, the coating compounded by the present application can not only have better compatibility and fit with the components after the immersion treatment, but also form an excellent network interweaving in the process of forming the coating, thereby forming a coating with significant waterproof and corrosion-resistant properties. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0020] A surface treatment method for an aluminum alloy battery tray in one embodiment of the present invention comprises the following steps:

[0021] The aluminum alloy battery tray is subjected to degreasing, alkaline etching and polishing treatment to obtain an aluminum alloy battery tray with a clean surface;

[0022] The aluminum alloy battery tray with a clean surface is soaked, dried and coated;

[0023] Among them, the immersion treatment is: immersing the aluminum alloy battery tray with a clean surface in a treatment solution prepared in advance, and the treatment solution includes nano sodium silicate, sodium molybdate, tin chloride and ammonium phosphate, and the concentration of nano sodium silicate is 5g / L~8g / L, sodium molybdate is 12g / L~20g / L, tin chloride is 9g / L~13g / L and ammonium phosphate is 7g / L~10g / L.

[0024] In one embodiment, the degreasing treatment is performed by adding trisodium phosphate, nonylphenol polyoxyethylene ether and sodium dodecyl sulfate into a mixed solution and heating the mixture to 45° C. to 65° C. for 20 min to 45 min.

[0025] In one embodiment, the concentration of trisodium phosphate is 80 g / L to 90 g / L, the concentration of nonylphenol polyoxyethylene ether is 5 mL / L to 6 mL / L, and the concentration of sodium dodecyl sulfate is 3 g / L to 5 g / L.

[0026] In one embodiment, the alkaline etching treatment uses sodium hydroxide with a concentration of 20g / L to 45g / L.

[0027] In one embodiment, the temperature of the alkaline etching treatment is 45° C. to 65° C., and the time is 30s to 50s.

[0028] In one embodiment, the immersion treatment temperature is 60°C to 85°C, the ultrasound-assisted frequency is 20kHz to 50kHz, and the time is 30min to 50min.

[0029] In one embodiment, the drying process is carried out in a nitrogen atmosphere at a temperature of 80° C. to 110° C. and for a time of 15 min to 30 min.

[0030] In one embodiment, the coating treatment is to apply a coating with a thickness of 30μm to 80μm on the surface of a dried aluminum alloy battery tray, and the coating includes the following preparation raw materials in parts by weight: 30 to 45 parts of ethylene oxide, 7 to 10 parts of titanium dioxide, 3 to 7 parts of sodium silicate, 7 to 11 parts of N,N-dimethylacrylamide, 1 to 20 parts of boron nitride particles and 2 to 7 parts of ethyl cellulose.

[0031] In one embodiment, the method for preparing the coating comprises the following steps: adding ethylene oxide, titanium dioxide, sodium silicate, N,N-dimethylacrylamide, boron nitride particles and ethyl cellulose into a stirring kettle, and stirring and mixing for 30 minutes to 60 minutes to obtain the coating.

[0032] In one embodiment, the average particle size of the boron nitride particles is 80 nm to 100 nm.

[0033] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0034] Embodiment 1:

[0035] A surface treatment method for an aluminum alloy battery tray comprises the following steps:

[0036] The aluminum alloy battery tray was added into a mixture of 80 g / L trisodium phosphate, 6 mL / L nonylphenol polyoxyethylene ether and 5 g / L sodium dodecyl sulfate and heated to 65°C for 20 min, then transferred to 65°C and 20 g / L sodium hydroxide for alkaline etching for 30 s, and then polished to obtain an aluminum alloy battery tray with a clean surface.

[0037] Prepare the treatment solution in the following proportions: 5g / L of nano sodium silicate, 12g / L of sodium molybdate, 13g / L of tin chloride and 10g / L of ammonium phosphate;

[0038] The aluminum alloy battery tray with a clean surface is transferred to the treatment liquid, immersed for 35 minutes at a temperature of 65°C and an ultrasonic-assisted frequency of 25kHz, then dried at 85°C for 15 minutes under a nitrogen atmosphere, and then coated with a coating with a thickness of 40 μm. The preparation method of the coating includes the following steps: 35 parts of ethylene oxide, 7 parts of titanium dioxide, 5 parts of sodium silicate, 9 parts of N,N-dimethylacrylamide, 11 parts of boron nitride particles and 5 parts of ethyl cellulose are added to a stirring kettle, and stirred and mixed for 35 minutes.

[0039] Embodiment 2:

[0040] A surface treatment method for an aluminum alloy battery tray comprises the following steps:

[0041] The aluminum alloy battery tray was added into a mixture of 85 g / L trisodium phosphate, 6 mL / L nonylphenol polyoxyethylene ether and 4 g / L sodium dodecyl sulfate and heated to 60°C for 25 min, then transferred to 50°C and 20 g / L sodium hydroxide for alkaline etching for 30 s, and then polished to obtain an aluminum alloy battery tray with a clean surface.

[0042] Prepare the treatment solution in the following proportions: 6 g / L of nano sodium silicate, 15 g / L of sodium molybdate, 10 g / L of tin chloride, and 8 g / L of ammonium phosphate;

[0043] The aluminum alloy battery tray with a clean surface is transferred to the treatment liquid, immersed for 30 minutes at a temperature of 75°C and an ultrasonic-assisted frequency of 25kHz, then dried at 85°C for 20 minutes under a nitrogen atmosphere, and then coated with a coating with a thickness of 40 μm. The preparation method of the coating includes the following steps: 40 parts of ethylene oxide, 10 parts of titanium dioxide, 5 parts of sodium silicate, 7 parts of N,N-dimethylacrylamide, 10 parts of boron nitride particles and 5 parts of ethyl cellulose are added to a stirring kettle, and stirred and mixed for 40 minutes.

[0044] Embodiment 3:

[0045] A surface treatment method for an aluminum alloy battery tray comprises the following steps:

[0046] The aluminum alloy battery tray was added into a mixture of 82 g / L trisodium phosphate, 6 mL / L nonylphenol polyoxyethylene ether and 5 g / L sodium dodecyl sulfonate and heated to 65°C for 20 min, then transferred to 65°C and 20 g / L sodium hydroxide for alkaline etching for 30 s, and then polished to obtain an aluminum alloy battery tray with a clean surface.

[0047] Prepare the treatment solution in the following proportions: 8 g / L of nano sodium silicate, 15 g / L of sodium molybdate, 11 g / L of tin chloride, and 8 g / L of ammonium phosphate;

[0048] The aluminum alloy battery tray with a clean surface is transferred to the treatment liquid, immersed for 35 minutes at a temperature of 75°C and an ultrasonic-assisted frequency of 30kHz, then dried at 85°C for 20 minutes under a nitrogen atmosphere, and then coated with a coating with a thickness of 40 μm. The preparation method of the coating includes the following steps: 35 parts of ethylene oxide, 8 parts of titanium dioxide, 5 parts of sodium silicate, 7 parts of N,N-dimethylacrylamide, 11 parts of boron nitride particles and 4 parts of ethyl cellulose are added to a stirring kettle, and stirred and mixed for 45 minutes.

[0049] Embodiment 4:

[0050] A surface treatment method for an aluminum alloy battery tray comprises the following steps:

[0051] The aluminum alloy battery tray was added into a mixture of 83 g / L trisodium phosphate, 6 mL / L nonylphenol polyoxyethylene ether and 4 g / L sodium dodecyl sulfonate and heated to 60°C for 23 min, then transferred to 65°C and 20 g / L sodium hydroxide for alkaline etching for 30 s, and then polished to obtain an aluminum alloy battery tray with a clean surface.

[0052] Prepare the treatment solution in the following proportions: 8 g / L of nano sodium silicate, 18 g / L of sodium molybdate, 9 g / L of tin chloride, and 7 g / L of ammonium phosphate;

[0053] The aluminum alloy battery tray with a clean surface is transferred to the treatment liquid, immersed for 35 minutes at a temperature of 80°C and an ultrasonic-assisted frequency of 25kHz, then dried at 85°C for 15 minutes under a nitrogen atmosphere, and then coated with a coating with a thickness of 40 μm. The preparation method of the coating includes the following steps: 35 parts of ethylene oxide, 8 parts of titanium dioxide, 7 parts of sodium silicate, 11 parts of N,N-dimethylacrylamide, 12 parts of boron nitride particles and 6 parts of ethyl cellulose are added to a stirring kettle, and stirred and mixed for 45 minutes.

[0054] Comparative Example 1:

[0055] Compared with Example 4, Comparative Example 1 was not subjected to alkaline etching treatment, and the rest was the same as Example 4.

[0056] Comparative Example 2:

[0057] Compared with Example 4, in Comparative Example 2, only single nano sodium silicate is added to the treatment liquid, and the rest is the same as Example 4.

[0058] Comparative Example 3:

[0059] Compared with Example 4, in Comparative Example 3, only sodium molybdate is added to the treatment liquid, and the rest is the same as Example 4.

[0060] Comparative Example 4:

[0061] Compared with Example 4, Comparative Example 4 is not subjected to immersion treatment, and the rest is the same as Example 4.

[0062] Comparative Example 5:

[0063] Compared with Example 4, Comparative Example 5 does not add sodium silicate to the coating of Comparative Example 5, and the rest is the same as Example 4.

[0064] Comparative Example 6:

[0065] Compared with Example 4, Comparative Example 6 does not add boron nitride particles to the coating of Comparative Example 6, and the rest is the same as Example 4.

[0066] The samples treated in Examples 1 to 4 and the comparative samples treated in Comparative Examples 1 to 6 were subjected to performance tests, and the results are shown in Table 1.

[0067] Adhesion is tested according to GB / T5210-2006; salt spray resistance is tested according to GB / T1771-2007.

[0068] The waterproof test uses an optical contact angle meter to measure the water contact angle of the sample surface at room temperature. When measuring the contact angle, a micro-syringe is used to measure a droplet of about 5 μL, and 5 different locations are selected on the surface of the aluminum alloy battery tray for measurement. The average value is taken as the contact angle value.

[0069] Table 1: Performance results

[0070]

[0071] From the data analysis in Table 1, it can be seen that after the surface treatment of the aluminum alloy battery tray in this application, the coating can have strong adhesion to the aluminum alloy surface, can fit more closely to the aluminum alloy surface, and is not easy to fall off. At the same time, after treatment, the surface of the aluminum alloy battery tray has significant corrosion resistance and waterproof effect, which helps to extend its service life.

[0072] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0073] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A surface treatment method for an aluminum alloy battery tray, characterized in that: The surface treatment method comprises the following steps: The aluminum alloy battery tray is subjected to degreasing, alkaline etching and polishing treatment to obtain an aluminum alloy battery tray with a clean surface; The aluminum alloy battery tray with a clean surface is soaked, dried and coated; Among them, the immersion treatment is: immersing the aluminum alloy battery tray with a clean surface in a treatment solution prepared in advance, and the treatment solution includes nano sodium silicate, sodium molybdate, tin chloride and ammonium phosphate, and the concentration of nano sodium silicate is 5g / L~8g / L, sodium molybdate is 12g / L~20g / L, tin chloride is 9g / L~13g / L and ammonium phosphate is 7g / L~10g / L.

2. The surface treatment method according to claim 1, characterized in that: The degreasing treatment is performed by adding trisodium phosphate, nonylphenol polyoxyethylene ether and sodium dodecyl sulfonate into a mixed solution and heating the mixture to 45° C. to 65° C. for 20 minutes to 45 minutes.

3. The surface treatment method according to claim 2, characterized in that: The concentration of trisodium phosphate is 80g / L to 90g / L, the concentration of nonylphenol polyoxyethylene ether is 5mL / L to 6mL / L, and the concentration of sodium dodecyl sulfate is 3g / L to 5g / L.

4. The surface treatment method according to claim 1, characterized in that: The alkaline etching treatment uses sodium hydroxide with a concentration of 20 g / L to 45 g / L.

5. The surface treatment method according to claim 4, characterized in that: The temperature of the alkali etching treatment is 45° C. to 65° C., and the time is 30s to 50s.

6. The surface treatment method according to claim 1, characterized in that: The immersion treatment temperature is 60° C. to 85° C., the ultrasound-assisted frequency is 20 kHz to 50 kHz, and the soaking time is 30 min to 50 min.

7. The surface treatment method according to claim 1, characterized in that: The drying process is carried out in a nitrogen atmosphere at a temperature of 80° C. to 110° C. and for a time of 15 min to 30 min.

8. The surface treatment method according to claim 1, characterized in that: The coating treatment is to apply a coating with a thickness of 30 μm to 80 μm on the surface of a dried aluminum alloy battery tray, and the coating includes the following preparation raw materials in parts by weight: 30 to 45 parts of ethylene oxide, 7 to 10 parts of titanium dioxide, 3 to 7 parts of sodium silicate, 7 to 11 parts of N,N-dimethylacrylamide, 1 to 20 parts of boron nitride particles and 2 to 7 parts of ethyl cellulose.

9. The surface treatment method according to claim 8, characterized in that: The preparation method of the coating comprises the following steps: adding ethylene oxide, titanium dioxide, sodium silicate, N,N-dimethylacrylamide, boron nitride particles and ethyl cellulose into a stirring kettle, and stirring and mixing for 30 minutes to 60 minutes to obtain the coating.

10. The surface treatment method according to claim 9, characterized in that: The average particle size of the boron nitride particles is 80nm to 100nm.

Citation Information

Patent Citations

  • Nanometer treatment technology of surface of aluminum alloy hub

    CN103506267A

  • Corrosion-resistant magnesium aluminum alloy chromium-free passivation solution

    CN104561970A

  • Anti-corrosion thermal conductive coating

    CN106609051A

  • Protective film for slowing corrosion of liquid metal on surface of aluminum alloy and preparation method of protective film

    CN109023334A

  • Nano film coating agent

    CN110819977A

Cited By

  • Surface treatment method of magnesium alloy battery tray

    CN120772113A