Method for synchronously removing sodium and potassium in aluminum-chromium slag dust by carbide slag mild hydrothermal method
Through the mild hydrothermal method of calcium carbide slag combined with calcium ion replacement and cation exchange resin recycling, Na2O and K2O in aluminum chromium slag dust were successfully removed, and the problem of aluminum chromium slag dust storage was solved, achieving efficient and low-cost resource utilization , suitable for industrial applications.
Patent Information
- Application Number
- CN202411278030.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The prior art is difficult to effectively remove Na2O and K2O from aluminum chromium slag dust at low cost and efficiently, resulting in the accumulation of these dusts, affecting the environment and economic benefits, and the calcium carbide slag has not been fully utilized.
By using the mild hydrothermal method of calcium carbide slag, the aluminum chromium slag dust is mixed with the calcium carbide slag aqueous solution, heat up and stir, filter and wash, and calcium ions are used to replace the insoluble alkali to achieve the removal of Na2O and K2O, and circulation is carried out through strong acid cation exchange resin. use.
The removal rate of Na2O in aluminum chromium slag dust reaches more than 90%, and the removal rate of K2O reaches more than 70%, which meets the composition requirements of chromium corundum high-grade refractory materials, and has strong process operability, low cost, and has industrial application prospects.
Smart Images

Figure CN118988953A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of industrial solid waste resource utilization, and relates to a method for synchronously removing sodium and potassium from aluminum-chromium slag dust by using a mild hydrothermal method with carbide slag. Background Art
[0002] Chromium is an important alloy element, mainly used to prepare high-temperature alloys, resistance alloys, precision alloys and other non-ferrous alloys. The aluminothermic method uses aluminum as a reducing agent to reduce chromium from chromium trioxide. Due to the violent reaction, a large amount of aluminum-chromium slag dust will be generated around the reactor and at the end of the dust removal system. In addition, a large amount of aluminum-chromium slag dust will be generated during the crushing of blocky aluminum-chromium slag. Aluminum-chromium slag has a high content of aluminum oxide and a certain amount of chromium oxide, and is widely used in the field of refractory materials. In the field of non-ferrous metallurgy, aluminum-chromium slag can be selected and crushed, and then pressed and sintered with a variety of auxiliary materials to prepare chrome corundum bricks, which are used in zinc smelting industrial kilns. In the field of iron and steel metallurgy, aluminum-chromium slag can be used as raw material to prepare blast furnace tapping ditch castables, medium frequency furnace ramming materials, and breathable bricks. At present, aluminum-chromium slag has been used in the fields of non-ferrous metallurgy and iron and steel metallurgy, and has achieved certain results, but some problems have also been encountered during its use. The aluminum-chromium slag dust produced by the above process contains a high level of alkali metal oxides such as Na2O and K2O. When the content of these alkali metal oxides exceeds a certain range, it will seriously affect the quality of refractory materials, such as refractoriness, strength, and service life. Therefore, relevant refractory material manufacturers have strict restrictions on the content of Na2O and K2O in aluminum-chromium slag. This leads to a large amount of dust containing excessive Na2O and K2O being stored and unable to be consumed, causing continuous harm to the environment and human body, and also affecting the economic benefits and storage costs of chromium production companies. Therefore, how to dealkalize aluminum-chromium slag dust at low cost and high efficiency has become a key technology to expand the utilization rate of aluminum-chromium slag dust.
[0003] Carbide slag mainly comes from the production of polyvinyl chloride and vinyl acetate by the calcium carbide process. About 1.45 tons of calcium carbide are consumed to produce 1 ton of polyvinyl chloride or vinyl acetate, and more than 1 ton of calcium carbide slag is produced after the hydrolysis of each ton of calcium carbide. Therefore, more than 2 tons of calcium carbide slag are required to be discharged for every ton of polyvinyl chloride or vinyl acetate produced. The amount of calcium carbide slag is large, and if it is discharged without treatment, it will clog the sewer, accumulate the riverbed, and endanger fishery production. Stacking it on land will occupy land and pollute the environment. If the solid waste of calcium carbide slag can be fully utilized and the Na and K in the aluminum-chromium slag dust can be removed simultaneously, it can provide a new way for low-pollution emissions and high-value resource utilization of aluminum-chromium slag dust and calcium carbide slag, thereby achieving the purpose of treating waste with waste and synergistic resource utilization of multiple solid wastes.
[0004] Therefore, how to develop a method for simultaneously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method of carbide slag is an urgent problem to be solved by technicians in this field. Summary of the invention
[0005] In view of this, the present invention provides a method for synchronously removing sodium and potassium from aluminum-chromium slag dust by using a mild hydrothermal method of carbide slag.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0008] (1) collecting aluminum chromium slag dust generated by the aluminothermic method for preparing metallic chromium for later use;
[0009] (2) fully dissolving the carbide waste residue produced when preparing polyvinyl chloride or vinyl acetate products by the carbide acetylene process in water to prepare a carbide slag aqueous solution;
[0010] (3) adding the aluminum-chromium slag dust in step (1) to the carbide slag aqueous solution in step (2), mixing well and then transferring to a reactor;
[0011] (4) The reactor is continuously stirred and heated, and after the temperature is kept warm, cooling water is turned on to cool the reaction slurry;
[0012] (5) After the reaction slurry in step (4) is cooled, it is filtered while hot, the solid-liquid separation is performed, and the obtained filter cake is washed with hot water, then filtered and dried.
[0013] Furthermore, the aluminum-chromium slag dust is one or a mixture of dust ash generated near the furnace mouth during the preparation of metallic chromium by the aluminothermic method, dust ash collected by a dust removal system, or dust generated during the crushing of blocky aluminum-chromium slag.
[0014] Furthermore, the aluminum-chromium slag dust and calcium carbide waste slag meet the required particle size requirement of ≤150 mesh without additional treatment and can be used directly.
[0015] Furthermore, the concentration of the carbide slag aqueous solution in step (2) is 16-20wt%, and the mass ratio of the aluminum-chromium slag dust to the carbide slag aqueous solution in step (3) is 1:(5-7).
[0016] The beneficial effects of adopting the above further technical solution are: ensuring the appropriate concentration of carbide slag and ensuring the subsequent treatment effect and efficiency.
[0017] Limiting the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution can ensure the appropriate ratio of Ca(OH)2 concentration brought into aluminum-chromium slag dust and carbide slag. It can avoid excessive carbide slag introducing impurities exceeding the standard, and avoid insufficient carbide slag, which cannot achieve efficient replacement of insoluble alkali.
[0018] Furthermore, the chemical composition of the aluminum-chromium slag dust requires Al2O3≥80wt%, Cr2O3≥13wt%, CaO≤0.30wt%, Fe2O3≤0.30wt%, MgO≤0.30wt%, SiO2≤0.30wt%; the chemical composition of the carbide slag requires CaO≥70wt%, Fe2O3≤0.30wt%, MgO≤0.30wt%, SiO2≤1.30wt%.
[0019] The beneficial effect of adopting the above further technical solution is that limiting the chemical composition requirements of aluminum-chromium slag dust can expand the sources of aluminum-chromium slag dust to be treated, and make its initial composition meet the requirements for the use of chrome corundum refractory materials.
[0020] Limiting the chemical composition of carbide slag ensures sufficient calcium source to meet the treatment concentration requirements, while avoiding excessive impurities that affect the quality of chrome corundum refractory materials.
[0021] Furthermore, in step (4), the reactor is heated at a rate of 5°C / min to 160-180°C, the insulation time is 90-120min, the stirring rate is 200 rpm, and the reaction pressure is 0.20-0.40MPa.
[0022] The beneficial effect of adopting the above further technical solution is that the structure of insoluble alkali (sodium and potassium) can be efficiently destroyed within the treatment condition range, so that Na and K enter the solution, providing a prerequisite for subsequent removal.
[0023] Furthermore, in step (5), when the reaction slurry of step (4) is cooled to 85-95°C, hot filtration and solid-liquid separation are started, and the obtained filter cake is washed 3-5 times with hot water at 85-95°C, and then filtered and dried to a water content of less than 3wt%.
[0024] The beneficial effect of adopting the above further technical solution is to ensure that the sodium and potassium ions entering the hot water solution can be fully washed away and avoid being adsorbed. Because when the temperature of the water solution is low, the Na and K in the solution will move back to the direction of generating insoluble alkali, affecting the removal effect.
[0025] Furthermore, in the step (5), the mass ratio of hot water used for each washing to the filter cake is (1.5-2.5):1.
[0026] Furthermore, the liquid phase after solid-liquid separation in step (5) and the liquid phase obtained after washing and filtration are uniformly collected, and then adsorbed by Tulsimer T-42H strong acid cation exchange resin, and the liquid phase can be returned to step (2) or step (5) for recycling.
[0027] The beneficial effects of adopting the above further technical solution are: saving water cost and achieving water recycling.
[0028] Furthermore, the chemical composition of the aluminum-chromium slag obtained after drying in step (5) is Al2O3≥80wt%, Cr2O3≥13wt%, CaO+MgO≤4.50wt%, Fe2O3≤0.45wt%, SiO2≤0.50wt%, Na2O≤0.25wt%, K2O≤0.75wt%, meeting the composition requirements for use of chrome corundum advanced refractory materials.
[0029] The beneficial effect of adopting the above further technical solution is to ensure that the composition requirements of high-grade chrome corundum refractory materials are met.
[0030] The beneficial effects of the present invention are as follows: the present invention utilizes the low-temperature and low-pressure hydrothermal method of calcium carbide slag to simultaneously remove Na2O and K2O from aluminum-chromium slag dust. The advantages of the present invention are that the temperature and pressure conditions of the present invention are relatively mild, and calcium carbide slag solid waste can be fully utilized to reduce the Na2O in the aluminum-chromium slag dust to below 0.25 and the K2O to below 0.75, thereby meeting the use requirements of chrome corundum high-grade refractory materials. At the same time, the reaction medium water solvent can be recycled in the system, and the industrial implementation is highly operable and the operating cost is low. This process achieves energy saving and consumption reduction and high-value utilization of aluminum-chromium slag dust, and is a dealkalization treatment process with low cost and large-scale industrial application prospects. The removal rate of Na2O reaches more than 90%, and the removal rate of K2O reaches more than 70%.
[0031] The technical concept of the present invention is that the potassium and sodium in the aluminum-chromium slag dust exist in the form of insoluble alkali and soluble alkali. The soluble alkali is removed by water leaching, while the insoluble alkali is basically difficult to remove by water leaching and is the main form of Na and K in the aluminum-chromium slag dust. Carbide slag contains rich calcium resources and can continuously provide Ca in the solution. 2+ Calcium ions can form precipitation with alkaline anions, thereby replacing sodium and potassium ions in insoluble alkalis, releasing them into the solution, and removing them through solid-liquid separation and multiple washings. 2+ The factors such as ion concentration (the amount of carbide slag added, the mass ratio of carbide slag solution to aluminum-chromium slag dust), temperature, system pressure, washing method, etc. are closely related. Under mild hydrothermal reaction conditions, i.e., a temperature range of 160-180°C, a heat preservation time of 90-120min, a system reaction pressure of 0.20-0.40MPa, and a washing hot water temperature of 85-95°C, the present invention uses carbide slag solid waste as a calcium source, which can effectively absorb carbide slag solid waste and remove potassium and sodium in aluminum-chromium slag dust, thereby achieving the synergistic high-value utilization of multiple solid wastes. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0036] (1) First, the dust generated near the furnace mouth during the preparation of metallic chromium by the aluminothermic method and the dust collected by the dust removal system are mixed evenly for later use. Then, the calcium carbide waste slag generated during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene method is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 18wt%.
[0037] Main raw material components: The aluminum-chromium slag dust obtained after uniform mixing has the following components: Cr2O3 13.42wt%, Al2O3 80.64wt%, CaO 0.15wt%, SiO2 0.26wt%, Fe2O3 0.15wt%, MgO 0.13wt%, Na2O 2.48wt%, K2O 2.53wt%, and others 0.24wt%.
[0038] The main components of calcium carbide waste slag are: CaO 71.28wt%, Fe2O30.15wt%, MgO 0.16wt%, SiO21.22wt%, Al2O31.75wt%, water content 24.23wt%, and others 1.21wt%.
[0039] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:5, and the mixture is fully stirred and then transferred to a reactor. Then the temperature is raised to 170°C at a heating rate of 5°C / min, the heat preservation time is 100min, the stirring rate during the whole process is 200 rpm, and the system reaction pressure is maintained at 0.30MPa. After the heat preservation time is up, the cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure, and stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 90°C, the reactor is opened, hot filtration is performed, solid-liquid separation is performed, and the obtained filter cake is repeatedly washed 4 times with 90°C hot water, and the mass ratio of the amount of hot water used for each washing to the filter cake is 2.0:1. After washing, suction filtration and drying are performed until the water content is less than 3wt%, and the aluminum-chromium slag after dealkalization is obtained.
[0040] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0041] (4) The aluminum-chromium slag dust obtained after drying contains 13.51 wt% Cr2O3, 80.58 wt% Al2O3, 4.05 wt% CaO, 0.49 wt% SiO2, 0.14 wt% Fe2O3, 0.14 wt% MgO, 0.22 wt% Na2O, 0.74 wt% K2O, and 0.12 wt% others. The removal rate of Na2O reaches 91.13%, and the removal rate of K2O reaches 70.75%.
[0042] Example 2
[0043] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0044] (1) First, the dust generated near the furnace mouth during the preparation of metallic chromium by the aluminothermic method and the dust collected during the crushing of the blocky aluminum chromium slag are mixed evenly for use. Then, the calcium carbide waste slag generated during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene method is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 20wt%.
[0045] Main raw material components: The aluminum-chromium slag dust obtained after uniform mixing has the following components: Cr2O3 13.71wt%, Al2O3 80.52wt%, CaO 0.14wt%, SiO2 0.22wt%, Fe2O3 0.14wt%, MgO 0.14wt%, Na2O 2.50wt%, K2O 2.51wt%, and others 0.22wt%.
[0046] The main components of calcium carbide waste slag are: CaO 70.32wt%, Fe2O30.16wt%, MgO 0.18wt%, SiO21.24wt%, Al2O31.86wt%, water content 24.91wt%, and others 1.33wt%.
[0047] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:6, and the mixture is fully stirred and then transferred to a reactor. Then the mixture is heated to 180°C at a heating rate of 5°C / min, and the heat preservation time is 90min. The stirring rate of the whole process is 200 rpm, and the system reaction pressure is maintained at 0.40MPa. After the heat preservation time is up, the cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure, and stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 95°C, the reactor is opened, and hot filtration is performed to separate the solid and liquid, and the obtained filter cake is repeatedly washed 3 times with 95°C hot water, and the mass ratio of the amount of hot water used for each washing to the filter cake is 2.5:1. After washing, the mixture is filtered and dried until the water content is less than 3wt%, and the aluminum-chromium slag after dealkalization is obtained.
[0048] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0049] (4) The aluminum-chromium slag dust obtained after drying contains 13.67 wt% Cr2O3, 80.46 wt% Al2O3, 4.16 wt% CaO, 0.41 wt% SiO2, 0.13 wt% Fe2O3, 0.13 wt% MgO, 0.19 wt% Na2O, 0.71 wt% K2O, and 0.14 wt% others. The removal rate of Na2O reaches 92.40%, and the removal rate of K2O reaches 71.71%.
[0050] Example 3
[0051] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0052] (1) First, the dust generated near the furnace mouth during the preparation of metallic chromium by the aluminothermic method and the dust collected by the dust removal system are mixed evenly for later use. Then, the calcium carbide waste slag generated during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene method is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 16wt%.
[0053] Main raw material components: The aluminum-chromium slag dust obtained after uniform mixing has the following components: Cr2O3 13.66wt%, Al2O3 80.34 wt%, CaO 0.16wt%, SiO2 0.26 wt%, Fe2O3 0.16 wt%, MgO 0.15wt%, Na2O 2.52wt%, K2O 2.54wt%, and others 0.21wt%.
[0054] The main components of calcium carbide waste slag are: CaO 71.93wt%, Fe2O30.14wt%, MgO 0.15wt%, SiO21.19wt%, Al2O31.81wt%, water content 23.54wt%, and others 1.24wt%.
[0055] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:7, and the mixture is fully stirred and then transferred to a reactor. Then the mixture is heated to 160°C at a heating rate of 5°C / min, the heat preservation time is 120min, the stirring rate during the whole process is 200 rpm, and the system reaction pressure is maintained at 0.20MPa. After the heat preservation time is up, cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure, and stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 85°C, the reactor is opened, hot filtration is performed, solid-liquid separation is performed, and the obtained filter cake is repeatedly washed 5 times with hot water at 85°C, and the mass ratio of the amount of hot water used for each washing to the filter cake is 1.5:1. After washing, suction filtration and drying are performed until the water content is less than 3wt%, and the aluminum-chromium slag after dealkalization is obtained.
[0056] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0057] (4) The aluminum-chromium slag dust obtained after drying contains 13.62 wt% Cr2O3, 80.29 wt% Al2O3, 4.21 wt% CaO, 0.40 wt% SiO2, 0.16 wt% Fe2O3, 0.16 wt% MgO, 0.23 wt% Na2O, 0.73 wt% K2O, and 0.13 wt% others. The removal rate of Na2O reaches 90.87%, and the removal rate of K2O reaches 71.26%.
[0058] Example 4
[0059] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0060] (1) First, the dust generated near the furnace mouth during the aluminothermic process for preparing metallic chromium, the dust collected by the dust removal system, and the dust collected during the crushing of the blocky aluminum chromium slag are mixed evenly for use. Then, the calcium carbide waste slag generated during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene process is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 17wt%.
[0061] Main raw material components: The aluminum-chromium slag dust obtained after uniform mixing has the following components: Cr2O3 13.22wt%, Al2O3 81.02 wt%, CaO 0.14wt%, SiO2 0.21 wt%, Fe2O3 0.13 wt%, MgO 0.13wt%, Na2O 2.47wt%, K2O 2.50wt%, and others 0.14wt%.
[0062] The main components of calcium carbide waste slag are: CaO 71.62wt%, Fe2O30.15wt%, MgO 0.16wt%, SiO21.23wt%, Al2O31.80wt%, water content 23.83wt%, and others 1.21wt%.
[0063] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:6.5, and the mixture is fully stirred and then transferred to a reactor. Then the mixture is heated to 175°C at a heating rate of 5°C / min, the heat preservation time is 95min, the stirring rate during the whole process is 200 rpm, and the system reaction pressure is maintained at 0.25MPa. After the heat preservation time is up, cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure, and stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 88°C, the reactor is opened, hot filtration is performed, solid-liquid separation is performed, and the obtained filter cake is repeatedly washed 4 times with hot water at 88°C, and the mass ratio of the amount of hot water used for each washing to the filter cake is 1.5:1. After washing, suction filtration and drying are performed until the water content is less than 3wt%, and the aluminum-chromium slag after dealkalization is obtained.
[0064] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0065] (4) The aluminum-chromium slag dust obtained after drying contains 13.15 wt% Cr2O3, 80.96 wt% Al2O3, 4.11 wt% CaO, 0.41 wt% SiO2, 0.14 wt% Fe2O3, 0.15 wt% MgO, 0.24 wt% Na2O, 0.74 wt% K2O, and 0.10 wt% others. The removal rate of Na2O reaches 90.28%, and the removal rate of K2O reaches 70.40%.
[0066] Example 5
[0067] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0068] (1) First, the dust dust obtained in the dust removal system during the preparation of metallic chromium by the aluminothermic method is collected for later use. Then, the calcium carbide waste residue produced during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene method is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 19 wt%.
[0069] Main raw material components: The contents of each component of dust ash are: Cr2O314.13 wt%, Al2O380.21 wt%, CaO0.12wt%, SiO20.20 wt%, Fe2O30.14 wt%, MgO 0.14wt%, Na2O 2.46wt%, K2O 2.49wt%, and others 0.11wt%.
[0070] The main components of calcium carbide waste slag are: CaO 70.38wt%, Fe2O30.16wt%, MgO 0.14wt%, SiO21.24wt%, Al2O31.79wt%, water content 25.11wt%, and others 1.18wt%.
[0071] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:5.5, and the mixture is fully stirred and then transferred to a reactor. Then the mixture is heated to 168°C at a heating rate of 5°C / min, the heat preservation time is 105min, the stirring rate during the whole process is 200 rpm, and the system reaction pressure is maintained at 0.35MPa. After the heat preservation time is up, the cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure, and stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 92°C, the reactor is opened, hot filtration is performed, solid-liquid separation is performed, and the obtained filter cake is repeatedly washed 3 times with 92°C hot water, and the mass ratio of the amount of hot water used for each washing to the filter cake is 2.5:1. After washing, suction filtration and drying are performed until the water content is less than 3wt%, and the aluminum-chromium slag after dealkalization is obtained.
[0072] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0073] (4) The aluminum-chromium slag dust obtained after drying contains 14.08 wt% Cr2O3, 80.16 wt% Al2O3, 4.04 wt% CaO, 0.42 wt% SiO2, 0.13 wt% Fe2O3, 0.13 wt% MgO, 0.21 wt% Na2O, 0.71 wt% K2O, and 0.11 wt% others. The removal rate of Na2O reaches 91.46%, and the removal rate of K2O reaches 71.49%.
[0074] Example 6
[0075] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0076] (1) First, the dust generated during the crushing of the blocky aluminum-chromium slag formed in the process of preparing metallic chromium by the aluminothermic method is collected for later use. Then, the calcium carbide waste slag generated during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene method is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 16wt%.
[0077] Main raw material components: The contents of the dust generated during the crushing of blocky aluminum-chromium slag are: Cr2O313.14wt%, Al2O381.15wt%, CaO 0.14wt%, SiO20.18wt%, Fe2O30.14wt%, MgO0.15wt%, Na2O 2.48wt%, K2O 2.53wt%, and others 0.09wt%.
[0078] The main components of calcium carbide waste slag are: CaO 71.96wt%, Fe2O30.17wt%, MgO 0.13wt%, SiO21.26wt%, Al2O31.82wt%, water content 23.48wt%, and others 1.18wt%.
[0079] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:5, and the mixture is fully stirred and then transferred to a reactor. Then the mixture is heated to 162°C at a heating rate of 5°C / min, the heat preservation time is 110min, the stirring rate during the whole process is 200 rpm, and the system reaction pressure is maintained at 0.25MPa. After the heat preservation time is up, cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure, and stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 85°C, the reactor is opened, hot filtration is performed, solid-liquid separation is performed, and the obtained filter cake is repeatedly washed 5 times with hot water at 85°C, and the mass ratio of the amount of hot water used for each washing to the filter cake is 1.5:1. After washing, suction filtration and drying are performed until the water content is less than 3wt%, and the aluminum-chromium slag after dealkalization is obtained.
[0080] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0081] (4) The aluminum-chromium slag dust obtained after drying contains 13.10 wt% Cr2O3, 81.13 wt% Al2O3, 4.05 wt% CaO, 0.43 wt% SiO2, 0.16 wt% Fe2O3, 0.13 wt% MgO, 0.19 wt% Na2O, 0.73 wt% K2O, and 0.08 wt% others. The removal rate of Na2O reaches 92.34%, and the removal rate of K2O reaches 71.15%.
[0082] Example 7
[0083] The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag comprises the following steps:
[0084] (1) First, the dust generated near the furnace mouth during the preparation of metallic chromium by the aluminothermic method is collected for later use. Then, the calcium carbide waste slag generated during the preparation of polyvinyl chloride and vinyl acetate products by the calcium carbide acetylene method is fully dissolved in water to prepare a calcium carbide slag aqueous solution with a concentration of 20wt%.
[0085] Main raw material components: The dust ash collected near the furnace mouth contains: Cr2O314.29 wt%, Al2O380.15 wt%, CaO 0.16wt%, SiO20.22 wt%, Fe2O30.14 wt%, MgO 0.14wt%, Na2O2.38wt%, K2O 2.42wt%, and others 0.10wt%.
[0086] The main components of calcium carbide waste slag are: CaO 70.28wt%, Fe2O30.16wt%, MgO 0.18wt%, SiO21.19wt%, Al2O31.76wt%, water content 25.18wt%, and others 1.25wt%.
[0087] (2) The aluminum-chromium slag dust mixed in step (1) is added to the carbide slag aqueous solution prepared in step (1), the mass ratio of aluminum-chromium slag dust to carbide slag aqueous solution is 1:7, and the mixture is fully stirred and then transferred to a reactor. Then the mixture is heated to 178°C at a heating rate of 5°C / min, and the heat preservation time is 95min. The stirring rate during the whole process is 200 rpm, and the system reaction pressure is maintained at 0.40MPa. After the heat preservation time is up, the cooling water is turned on to cool down, and the pressure relief valve is opened to release the system pressure. The stirring is stopped during the cooling process. When the temperature of the reaction slurry drops to 95°C, the reactor is opened, and the mixture is filtered while hot, solid-liquid separation is performed, and the obtained filter cake is repeatedly washed 3 times with hot water at 95°C, and the mass ratio of the amount of hot water used for each washing to the filter cake is 2.0:1. After washing, the mixture is filtered and dried until the water content is less than 3wt%, and the dealkalized aluminum-chromium slag is obtained.
[0088] (3) The liquid phase after solid-liquid separation and the liquid phase obtained after washing and filtration can be returned to the previous process requiring water solvent for recycling after adsorption by Tulsimer T-42H strong acid cation exchange resin.
[0089] (4) The aluminum-chromium slag dust obtained after drying contains 14.21 wt% Cr2O3, 80.12 wt% Al2O3, 4.05 wt% CaO, 0.35 wt% SiO2, 0.11 wt% Fe2O3, 0.14 wt% MgO, 0.22 wt% Na2O, 0.71 wt% K2O, and 0.09 wt% others. The removal rate of Na2O reaches 90.76%, and the removal rate of K2O reaches 70.66%.
[0090] Comparative Examples 1-6: Compared with Example 1, except for the reaction temperature, the other experimental raw materials and conditions of Comparative Examples 1-6 and Example 1 in step (2) are the same as those in Example 1. The removal rate data of Na2O and K2O are shown in Table 1 below.
[0091] Table 1 Reaction temperature and removal rate of Na2O and K2O in comparative examples 1-6
[0092] Comparative Example Reaction temperature <![CDATA[Na2O removal rate]]> <![CDATA[K2O removal rate]]> Comparative Example 1 140℃ 71.17% 50.91% Comparative Example 2 145℃ 77.41% 57.45% Comparative Example 3 150℃ 82.84% 62.73% Comparative Example 4 155℃ 87.23% 66.82% Comparative Example 5 185℃ 91.35% 70.96% Comparative Example 6 190℃ 91.51% 71.04%
[0093] Comparative Examples 7-11: Compared with Example 1, except for the difference in the holding time in step (2) of Example 1, other experimental raw materials and conditions are consistent with Example 1. The removal rate data of Na2O and K2O are shown in Table 2 below.
[0094] Table 2 Insulation time and removal rate of Na2O and K2O of comparative examples 7-11
[0095] Comparative Example Insulation time <![CDATA[Na2O removal rate]]> <![CDATA[K2O removal rate]]> Comparative Example 7 30min 67.21% 45.76% Comparative Example 8 50min 78.33% 58.82% Comparative Example 9 70min 86.62% 67.24% Comparative Example 10 140min 91.28% 70.91% Comparative Example 11 160min 91.46% 70.98%
[0096] Comparative Examples 12-16: Compared with Example 1, except for the difference in system reaction pressure in step (2) of Example 1, other experimental raw materials and conditions are consistent with Example 1. The removal rate data of Na2O and K2O are shown in Table 3 below.
[0097] Table 3 Reaction pressure of comparative examples 12-16 and removal rate of Na2O and K2O
[0098] Comparative Example System reaction pressure <![CDATA[Na2O removal rate]]> <![CDATA[K2O removal rate]]> Comparative Example 12 0.05MPa 70.12% 51.41% Comparative Example 13 0.10MPa 79.46% 61.25% Comparative Example 14 0.15MPa 85.93% 66.73% Comparative Example 15 0.45MPa 91.94% 71.36% Comparative Example 16 0.50MPa 92.08% 71.49%
[0099] Comparative Examples 17-21: Compared with Example 1, except for the difference in the temperature of the hot water used for washing the filter cake in step (2) of Example 1, other experimental raw materials and conditions are consistent with Example 1. The removal rate data of Na2O and K2O are shown in Table 4 below.
[0100] Table 4 Comparative Examples 17-21 Washing hot water temperature and removal rate of Na2O and K2O
[0101] Comparative Example Washing hot water temperature <![CDATA[Na2O removal rate]]> <![CDATA[K2O removal rate]]> Comparative Example 17 60℃ 73.55% 56.43% Comparative Example 18 70℃ 81.71% 62.32% Comparative Example 19 80℃ 87.62% 66.85% Comparative Example 20 98℃ 91.79% 71.29% Comparative Example 21 100℃ 91.87% 71.41%
[0102] The disclosed embodiments are described to enable one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for simultaneously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag, characterized in that: The following steps are involved: (1) collecting aluminum chromium slag dust generated by the aluminothermic method for preparing metallic chromium for later use; (2) fully dissolving the carbide waste residue produced when preparing polyvinyl chloride or vinyl acetate products by the carbide acetylene process in water to prepare a carbide slag aqueous solution; (3) adding the aluminum-chromium slag dust in step (1) to the carbide slag aqueous solution in step (2), mixing well and then transferring to a reactor; (4) The reactor is continuously stirred and heated, and after the temperature is kept warm, cooling water is turned on to cool the reaction slurry; (5) After the reaction slurry in step (4) is cooled, it is filtered while hot, the solid-liquid separation is performed, and the obtained filter cake is washed with hot water, then filtered and dried.
2. The method for simultaneously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 1, characterized in that: The aluminum-chromium slag dust is one or a mixture of dust generated near the furnace mouth during the preparation of metallic chromium by aluminothermic method, dust collected by a dust removal system, or dust generated during the crushing of blocky aluminum-chromium slag.
3. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method of carbide slag according to claim 1, characterized in that: The aluminum-chromium slag dust and calcium carbide waste slag meet the required particle size requirement of ≤150 mesh without additional treatment and can be used directly.
4. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 1, characterized in that: The concentration of the carbide slag aqueous solution in step (2) is 16-20wt%, and the mass ratio of the aluminum-chromium slag dust to the carbide slag aqueous solution in step (3) is 1:(5-7).
5. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 1, characterized in that: The chemical composition requirements of the aluminum-chromium slag dust are Al2O3≥80wt%, Cr2O3≥13wt%, CaO≤0.30wt%, Fe2O3≤0.30wt%, MgO≤0.30wt%, SiO2≤0.30wt%; the chemical composition requirements of the carbide slag are CaO≥70wt%, Fe2O3≤0.30wt%, MgO≤0.30wt%, SiO2≤1.30wt%.
6. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 1, characterized in that: In step (4), the reactor is heated at a rate of 5°C / min to 160-180°C, the insulation time is 90-120min, the stirring rate is 200 rpm, and the reaction pressure is 0.20-0.40MPa.
7. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 1, characterized in that: In step (5), when the reaction slurry of step (4) is cooled to 85-95°C, hot filtration and solid-liquid separation are started, and the obtained filter cake is washed 3-5 times with hot water at 85-95°C, and then filtered and dried to a water content of less than 3wt%.
8. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 7, characterized in that: In the step (5), the mass ratio of hot water used for each washing to the filter cake is (1.5-2.5):
1.
9. The method for synchronously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 7 or 8, characterized in that: The liquid phase after solid-liquid separation in step (5) and the liquid phase obtained after washing and filtration are collected uniformly, and then adsorbed by Tulsimer T-42H strong acid cation exchange resin, and the liquid phase can be returned to step (2) or step (5) for recycling.
10. The method for simultaneously removing sodium and potassium from aluminum-chromium slag dust by mild hydrothermal method using carbide slag according to claim 1, characterized in that: The chemical composition of the aluminum-chromium slag obtained after drying in step (5) is Al2O3≥80wt%, Cr2O3≥13wt%, CaO+MgO≤4.50wt%, Fe2O3≤0.45wt%, SiO2≤0.50wt%, Na2O≤0.25wt%, K2O≤0.75wt%, meeting the composition requirements for the use of chrome corundum advanced refractory materials.
Citation Information
Patent Citations
Process for Bayer process aluminum oxide production by replacing carbide slag with lime
CN101708859A
Dealkalization method of fly ash Al-extraction residues
CN102351451A
Method for removing sodium in vanadium-containing tailings under alkaline condition
CN105671327A
System and method for preparation of sulphoaluminate cement through collaboration of organic wastewater and industrial solid waste
CN106866006A
Method of producing zinc phosphate using phosphorus fertilizer
CN1830761A