Pelletizing treatment method of recycled powder and preparation method of thermal spraying target material

CN118989339APending Publication Date: 2024-11-22SHENZHEN APG MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115843.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing thermal spraying technology, the utilization rate of raw material powder and the inability to effectively recycle and reuse the residual target materials, resulting in high manufacturing costs and serious waste.

Method used

The recovery powder is pretreated by a combination of rolling and stirring granulation, and the fluidity is improved by friction and organic additive coating, and the particle diameter that meets the requirements of the spraying process is selected through multiple stirring and screening. The granulated powder in the range can realize the reuse of the powder.

Benefits of technology

It improves the utilization rate of raw material powder, reduces the production cost of thermally sprayed targets, realizes green circulation and low-cost manufacturing throughout the process, and ensures high deposition efficiency and quality of sprayed targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989339A_ABST
    Figure CN118989339A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of powder recovery, and provides a granulation treatment method of recovered powder and a preparation method of a thermal spraying target material. The granulation treatment method comprises the following steps: S1, squeezing the recycled powder, and then drying to obtain pretreated powder; s2, loading the pretreated powder into a stirring and granulating device, carrying out first stirring and granulating, and then screening to obtain first-particle-size granulated powder and second-particle-size granulated powder; s3, carrying out the following circulation process on the second particle size granulation powder: loading the second particle size granulation powder and the pretreated powder into a stirring granulation device, carrying out second stirring granulation, and then screening to obtain the first particle size granulation powder and the second particle size granulation powder; and S4, combining the granulation powder with the first particle size obtained in the step S2 and the step S3 as spraying powder for thermal spraying. According to the granulation treatment method, squeezing and stirring granulation are combined, the recycled powder can be granulated into uniform and compact granulation powder with good fluidity, the requirement for the thermal spraying process is met, and low-cost manufacturing is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of powder recovery, and in particular relates to a granulation processing method for recovered powder and a preparation method for thermal spraying target materials. Background Art

[0002] Thermal spraying technology has developed rapidly in recent years. It is a method that uses a heat source to heat the powder to a molten or semi-molten state, and sprays and deposits it onto the pre-treated substrate surface at a certain speed to form a coating. Thermal spray powder is very important in the thermal spray process. In addition to meeting the functional requirements of the coating, it must also meet the requirements of the thermal spraying process so that the powder can be smoothly, stably and evenly transported to the spraying flame. Therefore, the basic properties of the powder, such as morphology, sphericity, particle size, fluidity and bulk density, have an important influence on the deposition efficiency and quality of the thermal spray target.

[0003] The metal raw material powder purchased in the production and manufacturing is generally obtained by mechanical crushing or aerosolization, and the functional ceramic raw material powder is generally synthesized by chemical method. However, the metal or functional ceramic raw material powder obtained by these methods usually contains fine powder, and its morphology and fluidity are poor. Therefore, in order to ensure the deposition efficiency and the quality of the spray target, the raw material powder needs to be screened to screen out the raw material powder that meets the spraying process, and the raw material fine powder with small particle size, poor morphology and fluidity will be screened out. Although the metal raw material fine powder can be granulated into granulated powder with good fluidity by aerosolization + screening, the aerosol equipment is expensive and energy-consuming, so that the metal raw material fine powder that is screened out is usually treated as waste, resulting in low utilization rate of raw material powder and high manufacturing cost; the functional ceramic raw material fine powder can also be granulated into granulated powder with good fluidity by spray granulation, but the price of spray granulation equipment is relatively high, and there is also the problem of high target manufacturing cost.

[0004] At present, the utilization rate of sputtering targets is generally low, and the remaining targets (residual targets) are usually disposed of as waste at a very low price, which causes great waste, especially the residual targets whose raw material powder for sputtering targets is very expensive, which undoubtedly causes excessively high manufacturing costs.

[0005] Therefore, it is necessary to develop a granulation processing method for recycled powder to improve the utilization rate of raw powder and the recycling and reuse of residual targets, so as to achieve green circulation and low-cost manufacturing throughout the process. Summary of the invention

[0006] The purpose of the present application is to provide a granulation processing method for recycled powder and a method for preparing thermal spray targets, aiming to solve the problem of low utilization rate of raw powder used to prepare thermal spray targets and inability to better recycle and reuse residual targets, resulting in excessively high preparation costs for the entire process.

[0007] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0008] In a first aspect, the present application provides a granulation method for recycling powder, comprising the following steps:

[0009] S1: slurrying the recovered powder and then drying it to obtain pretreated powder;

[0010] S2: loading the pretreated powder into a stirring granulation device, performing a first stirring granulation, and then sieving to obtain a granulated powder with a first particle size and a granulated powder with a second particle size;

[0011] S3: subjecting the second particle size granulated powder to the following cycle: loading the second particle size granulated powder and the pretreated powder into the stirring granulation device, performing a second stirring granulation, and then sieving to obtain the first particle size granulated powder and the second particle size granulated powder;

[0012] S4: The granulated powders of the first particle size obtained in step S2 and step S3 are combined as spray powder for thermal spraying.

[0013] In a second aspect, the present application provides a method for preparing a thermal spraying metal target, comprising the following steps:

[0014] Providing raw material powder and / or spray powder obtained by the granulation method provided in the present application;

[0015] The raw material powder and / or the spraying powder are sprayed onto a backing tube by a thermal spraying process to obtain a thermal spraying target material;

[0016] Wherein, the particle size of the raw material powder is 45 to 125 μm.

[0017] Compared with the prior art, this application has the following beneficial effects:

[0018] The first aspect of the present application provides a granulation method for recycled powder, which first slurries the recycled powder. On the one hand, the edges and corners of the recycled powder are sheared off by friction, extrusion, etc., which helps to improve the fluidity of the granulated powder obtained by subsequent stirring and granulation. On the other hand, an organic additive is added to coat the recycled powder, which helps to bond with other organic additives during subsequent stirring and granulation to form a compact and uniform granulated powder. Then the pre-treated powder is loaded into the stirring granulation device for the first stirring granulation, and the first particle size granulation powder that meets the requirements of the thermal spraying process and the second particle size granulation powder that does not meet the requirements of the spraying process are sorted out by screening, and then the second particle size granulation powder that does not meet the requirements of the spraying process and the pre-treated powder are subjected to the second stirring granulation, and the first particle size granulation powder that meets the requirements of the thermal spraying process and the second particle size granulation powder that does not meet the requirements of the spraying process are sorted out by screening, so that the second particle size granulation powder that does not meet the requirements of the spraying process and the pre-treated powder are repeatedly subjected to the second stirring granulation and screening, then the first particle size granulation powder that is repeatedly screened out for the first time and the subsequent repeated screening can be combined as a spray powder for thermal spraying, thereby realizing the reuse of the recovered powder, improving the utilization rate of raw materials, and reducing the production cost of the target material. Therefore, the granulation treatment method of the present application adopts a combination of pulping and stirring granulation, which can granulate the recovered powder into a uniform, compact, surface-shaped and fluid granulation powder, which meets the thermal spraying process and can ensure that the thermal spray target has a high deposition efficiency and good quality. In addition, the required pulping and stirring granulation equipment is simple, low-cost, and suitable for industrial production, thus achieving green circulation and low-cost manufacturing throughout the entire process.

[0019] The preparation method of the thermal spray target material provided in the second aspect of the present application adopts a thermal spraying process to spray the raw material powder and / or the spray powder prepared by the granulation treatment method of the present application onto the back tube, so the manufacturing cost is low and it can ensure that the prepared thermal spray target material has a higher deposition efficiency and better quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 is the SEM image of the recovered powder;

[0022] Figure 2 This is a SEM image of the first coarse granulated powder obtained by the granulation treatment method for the recycled powder provided in Example A1 of the present application;

[0023] Figure 3This is a physical photo of the thermal spray target material prepared by the method for preparing the thermal spray target material provided in Example B1 of the present application. DETAILED DESCRIPTION

[0024] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0025] The first aspect of the embodiment of the present application provides a granulation method for recycling powder, comprising the following steps:

[0026] S1: slurrying the recovered powder and then drying it to obtain pretreated powder;

[0027] S2: loading the pretreated powder into a stirring granulation device, performing a first stirring granulation, and then sieving to obtain a granulated powder with a first particle size and a granulated powder with a second particle size;

[0028] S3: subjecting the second particle size granulated powder to the following cycle: loading the second particle size granulated powder and the pretreated powder into a stirring granulation device, performing a second stirring granulation, and then sieving to obtain the first particle size granulated powder and the second particle size granulated powder;

[0029] S4: The first particle size granulated powders obtained in step S2 and step S3 are combined as spray powder for thermal spraying.

[0030] The granulation processing method of recycled powder provided in the embodiment of the present application first slurries the recycled powder. On the one hand, the edges and corners of the recycled powder are sheared off by friction, extrusion, etc., which helps to improve the fluidity of the granulated powder obtained by subsequent stirring and granulation. On the other hand, organic additives are added to coat the recycled powder, which helps to bond with other organic additives during subsequent stirring and granulation to form a compact and uniform granulated powder. Then the pre-treated powder is loaded into the stirring granulation device for the first stirring granulation, and the first particle size granulation powder that meets the requirements of the thermal spraying process and the second particle size granulation powder that does not meet the requirements of the spraying process are sorted out by screening, and then the second particle size granulation powder that does not meet the requirements of the spraying process and the pre-treated powder are subjected to the second stirring granulation, and the first particle size granulation powder that meets the requirements of the thermal spraying process and the second particle size granulation powder that does not meet the requirements of the spraying process are sorted out by screening, so that the second particle size granulation powder that does not meet the requirements of the spraying process and the pre-treated powder are repeatedly subjected to the second stirring granulation and screening, then the first particle size granulation powder that is repeatedly screened out for the first time and the subsequent repeated screening can be combined as a spray powder for thermal spraying, thereby realizing the reuse of the recovered powder, improving the utilization rate of raw materials, and reducing the production cost of the target material. Therefore, the granulation treatment method of the present application adopts a combination of pulping and stirring granulation, which can granulate the recovered powder into a uniform, compact, surface-shaped and fluid granulation powder, which meets the thermal spraying process and can ensure that the thermal spray target has a high deposition efficiency and good quality. In addition, the required pulping and stirring granulation equipment is simple, low-cost, and suitable for industrial production, thus achieving green circulation and low-cost manufacturing throughout the entire process.

[0031] In practical applications, the pretreated powder in step S2 is only a portion of the pretreated powder obtained in step S1, and the remaining pretreated powder obtained in step S1 is used in step S3 for the second stirring granulation together with the second particle size granulation powder.

[0032] In an embodiment, the stirring granulation device includes a granulation barrel for containing pretreated powder and / or granulation powder of the second particle size and an agitator arranged in the granulation barrel; the inclination angles of the granulation barrel and the agitator relative to the horizontal plane are both 30 to 60°. The granulation barrel and the agitator are tilted at a certain angle relative to the horizontal plane, which is conducive to delivering the pretreated powder and / or granulation powder of the second particle size at the bottom and edge of the barrel to the agitator, thereby achieving the best granulation effect of the pretreated powder and / or granulation powder of the second particle size, thereby forming granulation powder with better uniformity, smooth edges and fluidity.

[0033] In the above step S1, the recovered powder is selected from metal powder or functional ceramic powder. Among them, the metal powder can include pure metal powder and alloy powder, and can be specifically selected from at least one of niobium powder, silver powder, tungsten titanium powder, titanium niobium powder, nickel chromium powder, copper nickel powder, zinc aluminum powder, zinc tin powder, molybdenum niobium powder, aluminum neodymium powder, aluminum cerium powder and aluminum scandium powder. These metal powders can be from metal powder raw materials prepared by crushing or atomization, and the metal raw material fine powder that does not meet the thermal spraying process is screened out, that is, the metal powder raw material with a particle size of less than 45μm; it can also be from the target material (residual target) that cannot be used after sputtering coating, and the pure metal crushed powder or alloy crushed powder is obtained after hydrogen crushing or mechanical crushing. Regardless of whether these metal powders come from metal powder raw materials or residual targets, they need to meet the oxygen content of less than 500ppm and the metal impurity content of less than 100ppm. The functional ceramic powder is selected from at least one of chromium carbide powder, titanium nitride powder, niobium oxide powder, molybdenum oxide powder, chromium oxide powder, titanium oxide powder, zirconium oxide powder and tantalum oxide powder. These functional ceramic powders can be obtained by air flow crushing of unusable target materials (residual targets) left over after sputtering coating, and the metal impurity content must be less than 100ppm.

[0034] In the embodiment, the particle size of the recovered powder is less than 45 μm. The recovered powder in this particle size range has poor fluidity, which makes it difficult to transport the powder and cannot meet the requirements of the spraying process. By adopting the granulation treatment method provided in the embodiment of the present application to perform slurry rolling, stirring granulation and screening, a granulated powder with uniform particle size distribution, compactness, good surface morphology and good fluidity can be obtained, which meets the requirements of the thermal spraying process and can be used to prepare thermal spray targets, thereby realizing green circulation and low-cost manufacturing throughout the entire process.

[0035] In an embodiment, when the recovered powder is selected from metal powder, the step of slurrying the recovered powder includes: slurrying the recovered powder and the first oily organic additive to form a slurry with a solid content of 85-95%. The first oily organic additive is selected from fatty acid methyl ester. Through slurrying, the fatty acid methyl ester forms a coating on the metal powder, which, on the one hand, prevents the metal powder from being oxidized, helps prevent the spray target from cracking, and forms a dense target. On the other hand, it helps the subsequent stirring granulation and bonding with the second oily organic additive to form a more compact and uniform granulated powder, thereby improving the fluidity of the granulated powder.

[0036] In the embodiment, the added amount of the first oily organic additive is less than or equal to 0.2% of the mass of the recovered powder.

[0037] In an embodiment, when the recovered powder is selected from functional ceramic powder, the step of slurrying the recovered powder includes: slurrying the recovered powder and the first aqueous organic additive to form a slurry with a solid content of 85 to 95%. Among them, the first aqueous organic additive is selected from polyethylene glycol. Through slurrying, polyethylene glycol forms a coating on the functional ceramic powder, which, on the one hand, promotes the spheroidization of the functional ceramic powder, makes the edge of the powder smoother, and helps to improve the fluidity of the granulated powder formed by subsequent stirring and granulation. On the other hand, it helps the subsequent stirring and granulation to bond with the second aqueous organic additive to form a more compact and uniform granulated powder, thereby improving the fluidity of the granulated powder.

[0038] In the embodiment, the added amount of the first aqueous organic additive is less than or equal to 0.5% of the mass of the recovered powder.

[0039] In the above step S2, the pre-treated powder is loaded into the stirring granulation device, which also includes: according to the mass ratio of the pre-treated powder to the solid plastic ball being 1 / (1-3), the pre-treated powder and the solid plastic ball are loaded into the stirring granulation device; wherein the solid plastic ball is composed of a first polyurethane ball, a second polyurethane ball and a third polyurethane ball in a mass ratio of 1 / (2-4) / (4-8), and the radii of the first polyurethane ball, the second polyurethane ball and the third polyurethane ball are 4-6μm, 8-12μm and 18-22μm respectively. Adding the solid plastic ball of this embodiment to impact the powder can prevent the use of an overly heavy metal ball or ceramic ball to impact the granulation powder and cause damage, so that the obtained granulation powder is compact, has a smooth morphology edge and good fluidity, which is conducive to improving the deposition efficiency and relative density of the sprayed metal target.

[0040] In the embodiment, the Shore hardness of the first polyurethane ball, the second polyurethane ball and the third polyurethane ball are independently 30-60A. During the stirring and granulating process, the hardness of the polyurethane ball has a certain influence on the powder, and the particle sizes of the granulated powder obtained by stirring and granulating polyurethane balls of different hardness are different. Therefore, under the cooperation of the Shore hardness range of the first polyurethane ball, the second polyurethane ball and the third polyurethane ball in this embodiment, it is more conducive to forming a granulated powder with a particle size of 45-125 μm.

[0041] In the embodiment, when the recovered powder is selected from metal powder, the first stirring granulation step includes: performing a first rotation process and a second rotation process on the granulation barrel and the stirrer, respectively, and spraying a second oily organic auxiliary agent solution into the pre-treated powder intermittently. The second oily organic auxiliary agent is selected from polyacrylic acid resin; in the first stirring granulation, the amount of the second oily organic auxiliary agent added is 0.1-0.3% of the mass of the pre-treated powder. This addition amount range can not only combine the pre-treated powder to form granulated powder, but also facilitate volatilization during the spraying process.

[0042] In an embodiment, when the recovered powder is selected from functional ceramic powder, the first stirring granulation step includes: performing a first rotation treatment and a second rotation treatment on the granulation barrel and the stirrer, respectively, and spraying the second aqueous organic auxiliary agent solution into the pretreated powder intermittently. The second aqueous organic auxiliary agent is selected from polyvinyl alcohol. In the first stirring granulation, the amount of the second aqueous organic auxiliary agent added is 0.1 to 0.3% of the mass of the pretreated powder. This addition amount range can not only combine the pretreated powder to form granulation powder, but also facilitate volatilization during the spraying process.

[0043] In the embodiment, the rotation direction of the first rotation treatment is opposite to that of the second rotation treatment; the rotation speed of the first rotation treatment is 50-150rpm, and the rotation speed of the second rotation treatment is 1000-2000rpm. For example: the first rotation treatment is a low-speed rotation in the clockwise direction, and the second rotation treatment is a high-speed rotation in the counterclockwise direction. In this embodiment, the pre-treated powder is stirred at high speed by the reverse motion between the granulation barrel rotating at low speed in the clockwise direction and the agitator rotating at high speed in the counterclockwise direction, and the second oily organic additive or the second aqueous organic additive solution is sprayed in at intervals at the same time. Under the joint action of the inclined granulation barrel, the pre-treated powder changes the movement direction to form a specific flow field, so that the pre-treated powder is "kneaded" to form nuclei during the high-speed movement, and then granulated into balls to form granulated powder.

[0044] In an embodiment, the step of screening the first coarse granulated powder obtained by the first stirring granulation may include: passing the first coarse granulated powder through a 120-mesh sieve and a 325-mesh sieve respectively to obtain a first particle size granulated powder with a particle size of 45 to 125 μm and a fluidity of 31 to 36 s / 50 g, and a second particle size granulated powder with a particle size of less than 45 μm.

[0045] In the above step S3, the second particle size granulation powder and the pre-treated powder are loaded into the stirring granulation device, which also includes: according to the mass ratio of the second particle size granulation powder, the pre-treated powder and the solid plastic ball is (0.2-0.5) / (0.5-0.8) / (1-3), the second particle size granulation powder, the pre-treated powder and the solid plastic ball are loaded into the stirring granulation device. The specific material and specification of the solid plastic ball in this step can be the same as that in step S2, and the mass ratio range is conducive to obtaining a compact granulation powder with smooth morphology and good fluidity, thereby helping to improve the deposition efficiency and relative density of the sprayed metal target.

[0046] In the embodiment, when the recovered powder is selected from metal powder, the second stirring granulation step includes: performing the third rotation process and the fourth rotation process on the granulation barrel and the stirrer respectively, and spraying the second oily organic auxiliary agent solution into the second particle size granulation powder and the pre-treated powder intermittently. Among them, the second oily organic auxiliary agent is selected from polyacrylic acid resin; in the second stirring granulation, the addition amount of the second oily organic auxiliary agent is 0.05-0.2% of the total mass of the second particle size granulation powder and the pre-treated powder, and the concentration of the second oily organic auxiliary agent solution is 5-20%. This addition amount range can not only combine the second particle size granulation powder and the pre-treated powder to form granulation powder, but also facilitate volatilization during the spraying process.

[0047] In an embodiment, when the recovered powder is selected from functional ceramic powder, the second stirring granulation step includes: performing a third rotation treatment and a fourth rotation treatment on the granulation barrel and the agitator, respectively, and at the same time, spraying the second aqueous organic auxiliary agent solution intermittently into the second particle size granulation powder and the pretreated powder. Among them, the second aqueous organic auxiliary agent is selected from polyvinyl alcohol. In the first stirring granulation, the addition amount of the second aqueous organic auxiliary agent is 0.05-0.1% of the total mass of the second particle size granulation powder and the pretreated powder, and the concentration of the second aqueous organic auxiliary agent solution is 5-20%. This addition amount range can not only combine the second particle size granulation powder and the pretreated powder to form granulation powder, but also facilitate volatilization during the spraying process.

[0048] In the embodiment, the rotation direction of the third rotation process is opposite to that of the fourth rotation process; the rotation speed of the third rotation process is 50-150rpm, and the rotation speed of the fourth rotation process is 1000-2000rpm. For example, the third rotation process is a low-speed clockwise rotation, and the fourth rotation process is a high-speed counterclockwise rotation. In this embodiment, the reverse motion between the granulation barrel rotating at a low speed in the clockwise direction and the agitator rotating at a high speed in the counterclockwise direction is used to stir the second particle size granulation powder and the pre-treated powder at a high speed, and the second oily organic additive or the second aqueous organic additive solution is sprayed intermittently at the same time. Under the joint action of the tilted granulation barrel, the second particle size granulation powder and the pre-treated powder change the movement direction to form a specific flow field, so that the second particle size granulation powder and the pre-treated powder are "kneaded" to form nuclei during the high-speed movement, and then granulated into balls to form granulation powder. In this way, the second particle size granulation powder that does not meet the spraying requirements is repeatedly subjected to a second stirring granulation and screening with the pretreated powder, and the granulation powder with suitable particle size, compactness, relatively smooth morphology edge and good fluidity is screened out as the spray powder for thermal spraying, thereby significantly improving the utilization rate of the raw material powder, realizing green circulation and low-cost manufacturing of the entire process.

[0049] In an embodiment, the step of screening the second coarse granulated powder obtained by the second stirring granulation may include: passing the second coarse granulated powder through a 120-mesh sieve and a 325-mesh sieve respectively to obtain a first particle size granulated powder with a particle size of 45 to 125 μm and a fluidity of 31 to 36 s / 50 g, and a second particle size granulated powder with a particle size of less than 45 μm.

[0050] In the embodiment, the number of cycles of the cycle process is 2 to 6. Through multiple cycles, the utilization rate of the raw materials can be improved, and the granulated powder with uniformity, compactness, smooth surface morphology and good fluidity can be obtained.

[0051] A second aspect of an embodiment of the present application provides a method for preparing a thermal spraying target, comprising the following steps:

[0052] Providing raw material powder and / or spray powder obtained by the granulation treatment method provided in the present application;

[0053] The raw material powder and / or the spraying powder are sprayed onto the backing tube by a thermal spraying process to obtain a thermal spraying target material;

[0054] The particle size of the raw material powder is 45-125 μm, and the raw material powder can be obtained by crushing or atomization preparation and passing through a 120-mesh sieve and a 325-mesh sieve respectively.

[0055] The method for preparing a thermal spray target provided in the embodiment of the present application uses a thermal spraying process to spray raw material powder and / or spray powder prepared by the granulation treatment method of the present application onto a backing tube, so the manufacturing cost is low and it can ensure that the prepared thermal spray target has a higher deposition efficiency and better quality.

[0056] In the embodiment, the spraying equipment includes a back tube and a spray gun, and the distance from the spray gun to the central axis of the back tube is 90 to 110 mm. If the distance between the spray gun and the central axis of the back tube is too long, the speed of the particles is reduced, the kinetic energy is reduced, and the bonding strength between the coatings and the coating and the back tube is reduced, which ultimately affects the density and strength of the target material obtained by spraying; if the distance between the spray gun and the central axis of the back tube is too short, the speed of the particles is too large, which easily causes powder splashing and reduces the deposition rate of the spray powder. Therefore, within the scope of this embodiment, the spray powder has a high deposition rate, high target density and high mechanical strength. The moving speed of the spray gun is 30 to 60 mm / min. This moving speed range allows the spray powder to be sprayed more evenly on the back tube, and the spray coating in some areas will not be too thick, thereby affecting the bonding strength between the coatings and the coating and the back tube.

[0057] In the embodiment, the powder feeding amount is 200-300 g / min. This powder feeding amount range can ensure a relatively high spraying efficiency while also facilitating the spray powder to be evenly sprayed onto the back tube to form a uniform and dense target material.

[0058] In the embodiment, the rotation speed of the back tube is 200-250 r / min. In this rotation speed range, the spray powder is sprayed on the back tube more evenly, and the coating is not too thick in some areas, thereby affecting the bonding strength between the coatings and between the coating and the back tube. The temperature of the back tube surface is 50-90°C.

[0059] The following describes the invention in conjunction with specific embodiments.

[0060] 1. Example of granulation method for recovered powder

[0061] Example A1

[0062] This embodiment provides a granulation method for niobium powder, comprising the following steps:

[0063] S11: using a three-roll mill to slurry the recovered niobium powder (particle size <45 μm, oxygen content less than 500 ppm, metal impurity content less than 100 ppm) and fatty acid methyl ester (added in an amount of 0.1% of the mass of the recovered niobium powder) to obtain a slurry with a solid content of 91%, and then drying the slurry to obtain pretreated niobium powder; wherein the recovered niobium powder is the metal niobium raw material powder with a particle size less than 45 μm that is screened out;

[0064] S12: according to the mass ratio of pretreated niobium powder to solid plastic balls being 1 / 2, part of the pretreated niobium powder and solid plastic balls are loaded into a granulation barrel of a stirring granulation device, the granulation barrel is rotated in a clockwise direction at a speed of 100 rpm, and the stirrer arranged in the granulation barrel stirs in a counterclockwise direction at a speed of 1500 rpm, and at the same time, a 15% polyacrylic acid resin solution (with pine alcohol as solvent) is sprayed into the pretreated niobium powder three times, and the mixture is stirred and granulated for 1.5 hours to obtain a first coarse granulation powder, which is then sieved through a 120-mesh sieve and a 325-mesh sieve to obtain a first particle size granulation powder (particle size of 45 to 125 μm) and a second particle size granulation powder (particle size <45 μm); wherein, the amount of polyacrylic acid resin added is 0.2% of the mass of the pretreated niobium powder, and the granulation barrel and the stirrer are inclined at 45° with respect to the horizontal plane;

[0065] S13: according to the mass ratio of the second particle size granulation powder, the pretreated niobium powder and the solid plastic balls being 0.3 / 0.7 / 2, the second particle size granulation powder, the pretreated niobium powder and the solid plastic balls are loaded into the granulation barrel of the stirring granulation device, the granulation barrel is rotated in the clockwise direction at a speed of 100 rpm, and the stirrer arranged in the granulation barrel is rotated in the counterclockwise direction at a speed of 1500 rpm, and at the same time, a polyacrylic acid resin solution with a concentration of 15% is sprayed into the second particle size granulation powder and the pretreated niobium powder three times, and the granulation is stirred and granulated for 1.5 hours to obtain a second coarse granulation powder, and then the second particle size granulation powder is respectively passed through a 120 mesh sieve and a 325 mesh sieve to obtain a first particle size granulation powder (particle size of 45 to 125 μm) and a second particle size granulation powder (particle size <45 μm); wherein the addition amount of the polyacrylic acid resin is 0.1% of the total mass of the second particle size granulation powder and the pretreated niobium powder;

[0066] The solid plastic ball is composed of a first polyurethane ball (particle size of 5 μm, Shore hardness of 45A), a second polyurethane ball (particle size of 10 μm, Shore hardness of 45A) and a third polyurethane ball (particle size of 20 μm, Shore hardness of 45A) in a mass ratio of 1 / 3 / 6;

[0067] S14: The first particle size granulated powders obtained in step S12 and step S13 are combined as spray powder for thermal spraying.

[0068] Example A2

[0069] This embodiment provides a granulation treatment method of titanium niobium powder, which is different from the embodiment A1 in that: recycled titanium niobium powder is used instead of recycled niobium powder;

[0070] The recovered titanium-niobium powder is obtained by hydrogen crushing and screening of titanium-niobium residual targets, in which the mass ratio of titanium to niobium is 1 / 1.

[0071] Example A3

[0072] This embodiment provides a granulation method for niobium oxide powder, which is different from embodiment A1 in that:

[0073] Replacing recycled niobium powder with recycled niobium oxide powder;

[0074] In step S11, the fatty acid methyl ester is replaced by polyethylene glycol (the addition amount is 0.3% of the mass of the recovered niobium oxide powder);

[0075] In steps S12 and S13, polyvinyl alcohol is used instead of polyacrylic acid resin.

[0076] Example A4

[0077] This embodiment provides a granulation method for niobium powder, which is different from the embodiment A1 in that:

[0078] In steps S12 and S13, no solid plastic balls are added during the stirring and granulation process.

[0079] Example A5

[0080] This embodiment provides a granulation method for niobium powder, which is different from the embodiment A1 in that:

[0081] In step S12, the mass ratio of the pretreated niobium powder and the solid plastic balls is 1 / 1;

[0082] In step S13, the mass ratio of the second particle size granulated powder, the pretreated niobium powder and the solid plastic balls is 0.5 / 0.5 / 1;

[0083] The solid plastic ball consists of a first polyurethane ball (particle size of 5 μm, Shore hardness of 30A), a second polyurethane ball (particle size of 10 μm, Shore hardness of 30A) and a third polyurethane ball (particle size of 20 μm, Shore hardness of 30A) in a mass ratio of 1 / 2 / 4.

[0084] Example A6

[0085] This embodiment provides a granulation method for niobium powder, which is different from the embodiment A1 in that:

[0086] In step S12, the mass ratio of the pretreated niobium powder to the solid plastic balls is 1 / 3;

[0087] In step S13, the mass ratio of the second particle size granulated powder, the pretreated niobium powder and the solid plastic balls is 0.2 / 0.8 / 3;

[0088] The solid plastic ball consists of a first polyurethane ball (particle size of 5 μm, Shore hardness of 60A), a second polyurethane ball (particle size of 10 μm, Shore hardness of 60A) and a third polyurethane ball (particle size of 20 μm, Shore hardness of 60A) in a mass ratio of 1 / 4 / 8.

[0089] Example A7

[0090] This embodiment provides a granulation method for niobium powder, which is different from the embodiment A1 in that:

[0091] In step S13, the second particle size granulated powder is subjected to the following two cycles: the second particle size granulated powder, the pretreated niobium powder and the solid plastic balls are loaded into the granulation barrel of the stirring granulation device according to the mass ratio of the second particle size granulated powder, the pretreated niobium powder and the solid plastic balls being 0.3 / 0.7 / 2, the granulation barrel is rotated in the clockwise direction at a speed of 100 rpm, the agitator arranged in the granulation barrel is rotated in the counterclockwise direction at a speed of 1500 rpm, and at the same time, a 15% polyacrylic acid resin solution is sprayed into the second particle size granulated powder and the pretreated niobium powder three times, the granulated powder is stirred and granulated for 1.5 hours, and then sieved through a 120 mesh sieve and a 325 mesh sieve respectively to obtain the first particle size granulated powder (particle size of 45 to 125 μm) and the second particle size granulated powder (particle size <45 μm).

[0092] Example A8

[0093] This embodiment provides a granulation method for niobium powder, which is different from the embodiment A1 in that:

[0094] In step S13, the second particle size granulated powder is subjected to the following 5 cycles: the second particle size granulated powder, the pretreated niobium powder and the solid plastic balls are loaded into the granulation barrel of the stirring granulation device according to the mass ratio of the second particle size granulated powder, the pretreated niobium powder and the solid plastic balls being 0.3 / 0.7 / 2, the granulation barrel is rotated in the clockwise direction at a speed of 100 rpm, the agitator arranged in the granulation barrel is rotated in the counterclockwise direction at a speed of 1500 rpm, and at the same time, a 15% polyacrylic acid resin solution is sprayed into the second particle size granulated powder and the pretreated niobium powder three times, the granulated powder is stirred and granulated for 1.5 hours, and then sieved through a 120 mesh sieve and a 325 mesh sieve respectively to obtain the first particle size granulated powder (particle size of 45 to 125 μm) and the second particle size granulated powder (particle size <45 μm).

[0095] Comparative Example A1

[0096] This comparative example provides a granulation method for niobium oxide powder, comprising the following steps:

[0097] S1: chemically synthesized niobium oxide raw material powder (particle size <45 μm, metal impurity content less than 100 ppm), polyethylene glycol (added in an amount of 0.3% by weight of the niobium oxide powder) and water are ball-milled and mixed, and then polyvinyl alcohol (added in an amount of 0.2% by weight of the niobium oxide powder) is added and mixed evenly to obtain a slurry;

[0098] S2: The slurry was introduced into a centrifugal spray granulator (inlet temperature: 180°C, outlet temperature: 100°C) for spray granulation to obtain granulated powder.

[0099] Comparative Example A2

[0100] This comparative example provides a granulation method for niobium powder, which differs from Example A1 in that:

[0101] This comparative example does not include step S11; in steps S12 and S13, the pre-treated niobium powder is replaced by the recovered niobium powder (that is, this comparative example does not perform slurry rolling on the recovered niobium powder, but directly stirs and granulates the recovered niobium powder).

[0102] Comparative Example A3

[0103] This comparative example provides a granulation method for niobium powder, which differs from Example A1 in that:

[0104] In steps S12 and S13, zirconia balls are used instead of solid plastic balls;

[0105] The zirconia balls consist of first zirconia balls (with a particle size of 5 μm), second zirconia balls (with a particle size of 10 μm) and third zirconia balls (with a particle size of 20 μm) in a mass ratio of 1 / 3 / 6.

[0106] Comparative Example A4

[0107] This comparative example provides a granulation method for niobium powder, which differs from Example A1 in that:

[0108] The first polyurethane ball, the second polyurethane ball and the third polyurethane ball all have a Shore hardness of 25A.

[0109] Comparative Example A5

[0110] This comparative example provides a granulation method for niobium powder, which differs from Example A1 in that:

[0111] The first polyurethane ball, the second polyurethane ball and the third polyurethane ball all have a Shore hardness of 65A.

[0112] 2. Example of Preparation Method for Thermal Spraying Target

[0113] Example B1

[0114] This embodiment provides a method for preparing a thermal spraying target, comprising the following steps:

[0115] S21: Weigh an appropriate amount of the spraying powder (metal niobium) obtained in Example A1;

[0116] S21: The treated back tube is installed on the frame, and the frame drives the back tube to rotate and move axially. The spray gun is installed 95mm above the central axis of the back tube. The rotation speed of the back tube is set to 220r / min, the moving speed of the spray gun is 40mm / min, the powder feeding amount is 250g / min, and the powder feeding gas and the working gas are both inert gases. During the spraying process, water is passed into the back tube to make the temperature of the back tube surface 75℃, and the spray powder is sprayed onto the back tube. The spraying is carried out for 6h to obtain a thermal spraying target.

[0117] Example B2

[0118] This embodiment provides a method for preparing a thermal spraying target material, which differs from Embodiment B1 in that:

[0119] In step S21, the spraying powder (metal niobium) obtained in Example A4 is used to replace the spraying powder (metal niobium) in Example A1.

[0120] Example B3

[0121] This embodiment provides a method for preparing a thermal spraying target material, which differs from Embodiment B1 in that:

[0122] In step S21, a proper amount of metal niobium raw material powder is weighed and passed through a 120-mesh sieve and a 325-mesh sieve respectively to obtain metal niobium raw material powder with a particle size of 45 to 125 μm as spray powder.

[0123] Example B4

[0124] This embodiment provides a method for preparing a thermal spraying target material, which differs from Embodiment B1 in that:

[0125] In step S21, the spray powder (niobium oxide) obtained in Example A3 is used to replace the spray powder (niobium metal) in Example A1.

[0126] Comparative Example B1

[0127] This comparative example provides a method for preparing a thermal spraying target material, which differs from Example B1 in that:

[0128] In step S21, the spray powder of Example A1 is replaced by the granulated powder (niobium oxide) obtained in Comparative Example A1.

[0129] Related performance test analysis:

[0130] 1. The recovered niobium powder (the metal niobium raw material powder that was screened out) and the first coarse granulated powder obtained in Example A1 were tested using a scanning electron microscope (SEM). The test results are as follows: Figures 1-2 shown.

[0131] from Figure 1 It can be seen that the particle size of the recycled niobium powder is less than 45μm, the size distribution is uneven and the sphericity is low, which cannot meet the requirements of the spraying process; Figure 2 It can be seen that the first coarse granulation powder is a compact granulation powder formed by combining several small-size recycled niobium powders. Its morphology edge is relatively smooth and the sphericity is good. After passing it through a 120-mesh sieve and a 325-mesh sieve, a granulation powder with a particle size in the range of 45 to 125 μm can be obtained, which meets the spraying process and can be used to prepare thermal spray targets. Figure 3 It can be seen that the thermal spraying target is uniform and dense.

[0132] 2. Use the following formula to calculate the recovery rate of the recovered powder:

[0133]

[0134] Wherein, n represents the second particle size granulation powder with a particle size less than 45 μm undergoing n cycles, and the calculation results are shown in Table 1 below.

[0135] 2. The particle size, powder fluidity and loose density of the spray powder recovered from Examples A1 to A8 of the present application and Comparative Examples A1 to A5 were tested using a Hall flow meter. The test results are shown in Table 1 below.

[0136] 3. The actual density of the thermal spraying targets prepared in Examples B1 to B4 of the present application and Comparative Example B1 was tested using the Archimedes density test method. The relative density was calculated based on the theoretical density. The test results are shown in Table 2 below.

[0137] Table 1

[0138] Implementation Recovery rate (%) <![CDATA[Bulk density (g / cm 3 )]]> D50(μm) Liquidity s / 50g Example A1 71.0 2.58 92.65 34.1 Example A2 71.4 1.84 92.74 33.3 Example A3 71.7 1.39 92.12 33.9 Example A4 70.8 2.31 92.46 31.7 Example A5 70.2 2.43 92.21 32.6 Example A6 70.4 2.48 91.75 32.8 Example A7 83.0 2.60 92.93 34.3 Example A8 92.6 2.62 93.22 34.6 Comparative Example A1 100 1.37 94.65 33.7 Comparative Example A2 53.7 2.37 83.18 30.2 Comparative Example A3 8.3 2.63 72.37 31.5 Comparative Example A4 65.0 2.46 85.46 26.9 Comparative Example A5 48.6 2.52 81.81 24.7

[0139] Table 2

[0140] Implementation Relative density (%) Example B1 92.75 Example B2 92.18 Example B3 93.20 Example B4 93.87 Comparative Example B1 94.01

[0141] As can be seen from Table 1, the spray powder (niobium oxide powder) obtained by granulation treatment in Example A3 has a D50 particle size of 92.12 μm, a fluidity of 33.9 s / 50 g, and a bulk density of 1.39 g / cm 3 Compared with the spray granulation method of Comparative Example A1, the difference is very small; the D50 particle size of the spray powder (niobium powder) obtained by granulation treatment of Examples A1, A4 to A8 is 91.75 to 93.22 μm, the fluidity is 31.7 to 34.6 s / 50 g, and the bulk density is 2.31 to 2.62 g / cm 3 ; It is explained that by using the granulation processing method for recycled powder provided in the embodiment of the present application to granulate the recycled powder, a compact granulated powder with uniform particle size distribution and good fluidity can be obtained, which can meet the requirements of the spraying process.

[0142] The loose density and fluidity of the spray powder of Example A1 are significantly better than those of Comparative Example A2 (without slurrying), indicating that the recycled powder is slurried in the embodiment of the present application and coated with an organic additive, which helps the subsequent stirring, granulation and bonding to form a more compact and uniform granulated powder. The edges and corners of the powder can also be sheared off to make the edge of the granulated powder smoother, thereby improving the fluidity of the granulated powder.

[0143] The loose density, fluidity and recovery rate of the spray powder of Example A1 are significantly better than those of Comparative Example A3 (using zirconia balls), indicating that the embodiment of the present application uses solid plastic balls to stir and granulate the powder. The impact of the solid plastic balls on the powder is beneficial to smoothing the edges and corners of the powder to obtain a more compact granulated powder with smoother edges and better fluidity, and prevents the use of heavy and hard metal balls or ceramic balls to impact the granulated powder and cause breakage, thereby reducing the recovery rate of the spray powder.

[0144] The recovery rates of the recovered powders in Examples A1 to A8 are all greater than 70%, and as the number of times the second particle size granulated powder is recycled increases, the recovery rate of the recovered powder increases significantly (such as Examples A1, A7 and A8). When the second particle size granulated powder is recycled 5 times, the recovery rate of the waste niobium powder can be as high as 92.6%, indicating that the granulation treatment method for the recovered powder provided in the embodiment of the present application has a high recycling rate for the recovered powder. And because the recovered powder can be either the raw material fine powder that is sieved out or the powder obtained by hydrogen crushing or mechanical crushing and sieving the residual target, the granulation treatment method for the recovered powder of the present application can achieve green circulation and low-cost manufacturing of the entire process.

[0145] As can be seen from Table 2, the relative density of the thermal spray target prepared by Examples B1, B2 and B4 is above 92.18, indicating that the thermal spray target prepared by the spray powder obtained by the granulation treatment method provided in the embodiment of the present application has a high relative density. In addition, the relative density of the thermal spray target prepared by Example B1 and Example B3 (using metal niobium raw material powder for spraying) is very small, and the relative density of the thermal spray target prepared by Example B4 and Comparative Example B1 (using spray granulation powder) is also very small, indicating that the spray powder obtained by the granulation treatment method provided in the embodiment of the present application can replace the metal raw material powder or spray granulation powder, and can also be used together with the metal raw material powder or spray granulation powder, so that low-cost manufacturing is achieved while ensuring the quality of the prepared target.

[0146] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A granulation method for recovering powder, It is characterized in that The following steps are involved: S1: slurrying the recovered powder and then drying it to obtain pretreated powder; S2: loading the pretreated powder into a stirring granulation device, performing a first stirring granulation, and then sieving to obtain a granulated powder with a first particle size and a granulated powder with a second particle size; S3: subjecting the second particle size granulated powder to the following cycle: loading the second particle size granulated powder and the pretreated powder into the stirring granulation device, performing a second stirring granulation, and then sieving to obtain the first particle size granulated powder and the second particle size granulated powder; S4: The granulated powders of the first particle size obtained in step S2 and step S3 are combined as spray powder for thermal spraying.

2. The granulation method according to claim 1, It is characterized in that The recycled powder is selected from metal powder and / or functional ceramic powder.

3. The granulation method according to claim 2, It is characterized in that When the recycled powder is selected from metal powder, the step of slurrying the recycled powder comprises: slurrying the recycled powder and the first oily organic additive to form a slurry with a solid content of 85-95%; Alternatively, when the recycled powder is selected from functional ceramic powder, the step of slurrying the recycled powder comprises: slurrying the recycled powder and the first aqueous organic additive to form a slurry with a solid content of 85-95%.

4. The granulation method according to claim 3, It is characterized in that At least one of the following conditions is met: The first oily organic additive is selected from fatty acid methyl esters; The first aqueous organic auxiliary agent is selected from polyethylene glycol; The metal powder is selected from at least one of niobium powder, silver powder, tungsten titanium powder, titanium niobium powder, nickel chromium powder, copper nickel powder, zinc aluminum powder, zinc tin powder, molybdenum niobium powder, aluminum neodymium powder, aluminum cerium powder and aluminum scandium powder; The functional ceramic powder is selected from at least one of chromium carbide powder, titanium nitride powder, niobium oxide powder, molybdenum oxide powder, chromium oxide powder, titanium oxide powder, zirconium oxide powder and tantalum oxide powder.

5. The granulation method according to any one of claims 1 to 4, It is characterized in that The method further comprises: charging the pretreated powder and the solid plastic balls into the stirring granulation device according to a mass ratio of the pretreated powder and the solid plastic balls of 1 / (1-3); And / or, the second particle size granulation powder and the pretreated powder are loaded into the stirring granulation device, which also includes: according to the mass ratio of the second particle size granulation powder, the pretreated powder and the solid plastic balls being (0.2-0.5) / (0.5-0.8) / (1-3), the second particle size granulation powder, the pretreated powder and the solid plastic balls are loaded into the stirring granulation device.

6. The granulation method according to claim 5, It is characterized in that The solid plastic ball is composed of a first polyurethane ball, a second polyurethane ball and a third polyurethane ball in a mass ratio of 1 / (2-4) / (4-8); The radii of the first polyurethane ball, the second polyurethane ball and the third polyurethane ball are 4-6 μm, 8-12 μm and 18-22 μm respectively, and the Shore hardness is independently 30-60A.

7. The granulation method according to claim 1, It is characterized in that The stirring granulation device comprises a granulation barrel for containing the pre-treated powder and / or the granulation powder of the second particle size and a stirrer arranged in the granulation barrel; When the recycled powder is selected from metal powder, the first stirring granulation step comprises: performing a first rotation process and a second rotation process on the granulation barrel and the stirrer, respectively, and intermittently spraying a second oily organic auxiliary agent solution into the pretreated powder; the second stirring granulation step comprises: performing a third rotation process and a fourth rotation process on the granulation barrel and the stirrer, respectively, and intermittently spraying a second oily organic auxiliary agent solution into the second particle size granulation powder and the pretreated powder; Alternatively, when the recycled powder is selected from functional ceramic powder, the first stirring granulation step includes: subjecting the granulation barrel and the agitator to a first rotation treatment and a second rotation treatment, respectively, and intermittently spraying a second aqueous organic auxiliary agent solution into the pretreated powder; the second stirring granulation step includes: subjecting the granulation barrel and the agitator to a third rotation treatment and a fourth rotation treatment, respectively, and intermittently spraying a second aqueous organic auxiliary agent solution into the second particle size granulation powder and the pretreated powder.

8. The granulation method according to claim 7, It is characterized in that At least one of the following conditions is met: In the first stirring granulation, the amount of the second oily organic additive or the second aqueous organic additive added is 0.1 to 0.3% of the mass of the pretreated powder; In the second stirring granulation, the amount of the second oily organic additive or the second aqueous organic additive added is 0.05-0.2% of the total mass of the second particle size granulation powder and the pretreated powder; The second oily organic additive is selected from polyacrylic acid resin; The second aqueous organic additive is selected from polyvinyl alcohol; The rotation direction of the first rotation process is opposite to the rotation direction of the second rotation process; The rotation direction of the third rotation process is opposite to the rotation direction of the fourth rotation process; The rotation speeds of the first rotation process and the third rotation process are both 50-150 rpm; The rotation speeds of the second rotation process and the fourth rotation process are both 1000-2000 rpm; The inclination angles of the granulation barrel and the agitator relative to the horizontal plane are both 30-60°.

9. The granulation method according to claim 1, It is characterized in that The first particle size granulated powder has a particle size of 45 to 125 μm and a fluidity of 31 to 36 s / 50 g; and / or, the particle sizes of the second particle size granulated powder and the recovered powder are both less than 45 μm; And / or, the number of cycles of the cyclic process is 2 to 6 times.

10. A method for preparing a thermal spraying target, It is characterized in that The following steps are involved: Providing raw material powder and / or spray powder obtained by the granulation treatment method according to any one of claims 1 to 9; The raw material powder and / or the spraying powder are sprayed onto a backing tube by a thermal spraying process to obtain a thermal spraying target material; Wherein, the particle size of the raw material powder is 45 to 125 μm.