Preparation method of large-size high-temperature alloy annular piece with controllable grain size

High-temperature alloy powder was prepared by high-speed plasma rotary electrode method and thermal isostatic pressing and rolling, which solved the problem of difficult grain size control of high-temperature alloy ring parts in traditional technology, and achieved high-performance and stable large-size high-temperature alloys Preparation of ring parts.

CN118989343AInactive Publication Date: 2024-11-22SINO EURO MATERIALS TECH OF XIAN CO LTD

Patent Information

Application Number
CN202411031884.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional forging and emerging additive manufacturing technologies are difficult to effectively control the grain size of high-temperature alloy rings, resulting in unstable performance, especially during the preparation of large-size rings.

Method used

High-speed plasma rotary electrode method is used to prepare high-temperature alloy metal spherical powder, and the powder with the desired particle size range is obtained through sieving, and hot isostatic pressure and fire rolling are carried out, combined with machining, and finally the required size and grains are obtained. high temperature alloy ring parts.

Benefits of technology

The fine control of the grain size of high-temperature alloy ring parts is achieved, performance stability and batch stability are improved, process flow is simplified, and segregation behaviors during multiple upsetting and remelting are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989343A_ABST
    Figure CN118989343A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of powder metallurgy, and particularly relates to a preparation method of a large-size high-temperature alloy annular piece with a controllable grain size. The method comprises the following steps: determining a grain size range according to performance requirements of a formed part, selecting powder materials of different grain size sections, and performing hot isostatic pressing to obtain original near-net ring blanks of different grain sizes; compared with a traditional as-cast bar, the structure distribution of the blank can be directly controlled according to the particle size of the powder, the controllability is high, and the batch stability is high; according to the near-net forming design, the ring blank subjected to hot isostatic pressing is obtained only through one-heating-number rolling deformation, repeated upsetting ring rolling is not needed, the production procedure is short, and the process technology is controllable; the ring blank used in the method is formed through powder diffusion sintering, the casting or additive manufacturing (3D printing) remelting process is not needed, the structure is uniform, segregation behaviors do not exist, and the high performance of a workpiece is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and relates to a method for preparing a high-temperature alloy ring part, and specifically relates to a method for preparing a large-size high-temperature alloy ring part with controllable grain size. Background Art

[0002] High-temperature alloy refers to a type of metal material based on iron, nickel and cobalt, which can work for a long time at high temperatures above 600°C and under certain stresses. It also has excellent high-temperature strength, good oxidation resistance and thermal corrosion resistance, good fatigue performance, fracture toughness and other comprehensive properties. Therefore, it is also called "superalloy" and is mainly used in the aerospace and energy fields.

[0003] During the preparation of high-temperature alloys, the microstructure will affect the mechanical properties of the high-temperature alloy, and the grain size has a certain influence on the mechanical properties, durability and high-temperature stability of the material. In daily production, high-temperature alloys with different grain size requirements are often required according to the use conditions and the alloys used; since the grain size has a significant effect on the mechanical properties of high-temperature alloys, it is necessary to pay attention to the selection of grain size when preparing high-temperature alloys. According to the use conditions, the grain size of high-temperature alloys is often controlled. For example, in a rotating use environment, the alloy grain size is required to be finer, and the strength and fatigue creep properties of the alloy are greatly improved; however, in conventional load-bearing component applications, the alloy's high-temperature plasticity and durability requirements are higher, and the corresponding grain size is a coarser grain size.

[0004] However, traditional forging, casting and emerging additive manufacturing technology (3D printing) have limited control over grain size, and it is difficult to obtain formed parts with the required grain size, especially rings. This is because in the traditional forging process, due to repeated forging, uneven firing and deformation will aggravate the recovery of the material grain size and uneven recrystallization, resulting in uneven grain size and unstable performance of the ring. For the emerging 3D printing technology, the material is remelted and solidified, and the grain production presents a columnar crystal morphology, and the grain size cannot be controlled. However, the existing technology still has the following problems in controlling grain size:

[0005] 1) The traditional forging process is to process large-sized cast bars through multiple rounds of upsetting, punching, multiple rounds of stamping, heat treatment and machining to obtain the final size of the ring. This method has many forging rounds and can only obtain a finer grain size according to the deformation amount. Moreover, the grain size is greatly different from the forming rounds, the forming shape and other factors, so it is difficult to control the grain size.

[0006] 2) Casting and the emerging additive manufacturing (3D printing) technology are both processes of remelting the metal and then cooling it into shape. The cooling rate and process temperature of the material will affect the microstructure. Therefore, the grain size of this process is also uncontrollable.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art and provide a method for preparing a large-sized high-temperature alloy ring with controllable grain size.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] A method for preparing a large-sized high-temperature alloy ring with controllable grain size, specifically comprising the following steps:

[0011] S1. Prepare a high-temperature alloy metal spherical powder by a high-speed plasma rotating electrode preparation method. Screen the prepared powder according to the final grain size requirements to select the required particle size range, wherein the upper and lower limit difference of the powder screening particle size screen is controlled within 70 μm, and the median particle size D50 of the powder laser particle size is controlled between 10 μm and 300 μm;

[0012] S2. After the original formed part size is reduced by 10% to 20% in proportion, the annular cavity thin-walled sheath is designed according to the reduced size, and the sheath shell is spliced ​​and welded according to the designed shape; the annular part cavity thickness formed by the sheath is 30mm to 1000mm, the outer diameter is 50mm to 1500mm, and the annular part height is 10mm to 2000mm; the sheath is made of 45# low carbon steel;

[0013] S3, the powder selected in S1 is loaded into the ring sleeve welded in S2, and after the powder is filled, it is vibrated, the vibration frequency is 30Hz~50Hz, and the amplitude is 1mm~5mm; the degassing pipe and the sleeve are argon arc welded and vacuumed, and the sleeve is heated to 200℃~500℃ and kept warm for ≥5h. When the vacuum degree is ≤3.5×10-3Pa, the degassing pipe is clamped and the sleeve is sealed; the size of the degassing pipe is Φ5~Φ30mm in diameter and 1000mm~2500mm in length, and the material is 20# steel;

[0014] S4, hot isostatic pressing the ring sleeve after sealing and welding, wherein the hot isostatic pressing temperature is 1090°C to 1410°C, the hot isostatic pressing pressure is 115MPa to 205MPa, and the hot isostatic pressing time is 1h to 5h; after completion, cooling with the furnace, the cooling rate is ≤15°C / min;

[0015] S5, machining the cooled ring sheath to remove the ring sheath on the surface to obtain a high-temperature alloy ring blank or a special-shaped ring blank;

[0016] S6, heating and keeping the obtained ring blank, wherein the heating temperature is 1090° C. to 1210° C., and the keeping time is 1 h to 2 h;

[0017] S7, rolling the heat-insulated ring blank once to obtain a thin-walled ring, designing a corresponding rolling die according to the size, and then fitting the thin-walled ring blank into the rolling die for rotational rolling, wherein the rolling deformation is 10% to 20%, and the rolling strain rate is 0.03s -1 ~0.1s -1 , rolling temperature range is 1000℃~1200℃;

[0018] S8, subjecting the rolled ring to a solution + aging heat treatment, wherein the solution temperature is 990°C to 1210°C, the holding time is 1h to 2h, and air cooling; the aging temperature is 740°C to 910°C, and the holding time is 7h to 8h;

[0019] S9. Machining the heat-treated ring to obtain a high-temperature alloy ring of a desired size.

[0020] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0021] 1) According to the performance requirements of the formed part, the grain size range is determined, powder materials of different grain sizes are selected, and hot isostatic pressing is performed to obtain original near-net ring blanks of different grain sizes; compared with traditional cast bars, the present invention can directly control the microstructure distribution of the blank according to the powder particle size, with strong controllability and high batch stability;

[0022] 2) According to the near-net-shape design, the ring blank after hot isostatic pressing is only deformed by one rolling process, and multiple upsetting ring rolling processes are not required. The production process is short and the process technology is controllable.

[0023] 3) The ring blank used in the present invention is formed by powder diffusion sintering without casting or additive manufacturing (3D printing) remelting process, and has uniform structure and no segregation behavior, thereby ensuring the high performance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0026] Figure 1It is a flow chart of the method for preparing a large-sized high-temperature alloy ring with controllable grain size according to the present invention;

[0027] Figure 2 The morphology of the GH4169 powder of 15 μm to 53 μm (D50: 25 μm) in Example 1;

[0028] Figure 3 The metallographic structure of the GH4169 ring with a grain size of 7 to 8 in Example 1;

[0029] Figure 4 The morphology of the GH4169 powder of 53 μm to 106 μm (D50: 67 μm) in Example 2;

[0030] Figure 5 The metallographic structure of the GH4099 ring with a grain size of 5 to 6 in Example 2;

[0031] Figure 6 The morphology of the GH4169 powder of 90 μm to 180 μm (D50: 110 μm) in Example 3;

[0032] Figure 7 This is the metallographic structure morphology of the GH4169 ring with grain size 3 to 4 in Example 3. DETAILED DESCRIPTION

[0033] Here, exemplary embodiments will be described in detail, and examples thereof are shown in the accompanying drawings. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention as detailed in the appended claims.

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0035] A method for preparing a large-sized high-temperature alloy ring with controllable grain size, specifically comprising the following steps:

[0036] S1. Prepare a high-temperature alloy metal spherical powder by a high-speed plasma rotating electrode preparation method. Screen the prepared powder according to the final grain size requirements to select the required particle size range, wherein the upper and lower limit difference of the powder screening particle size screen is controlled within 70 μm, and the median particle size D50 of the powder laser particle size is controlled between 10 μm and 300 μm;

[0037] S2. After the original formed part size is reduced by 10% to 20% in proportion, the annular cavity thin-walled sheath is designed according to the reduced size, and the sheath shell is spliced ​​and welded according to the designed shape; the annular part cavity thickness formed by the sheath is 30mm to 1000mm, the outer diameter is 50mm to 1500mm, and the annular part height is 10mm to 2000mm; the sheath is made of 45# low carbon steel;

[0038] S3. Load the powder selected in S1 into the ring sleeve welded in S2, and vibrate it after it is full, with a vibration frequency of 30Hz~50Hz and an amplitude of 1mm~5mm; perform argon arc welding on the degassing pipe and evacuate the sleeve, and heat the sleeve at 200℃~500℃ and keep it warm for ≥5h. When the vacuum degree is ≤3.5×10-3Pa, seal the degassing pipe; the size of the degassing pipe is Φ5~Φ30mm in diameter and 1000mm~2500mm in length, and the material is 20# steel.

[0039] S4, hot isostatic pressing the ring sleeve after sealing and welding, wherein the hot isostatic pressing temperature is (1100°C-1400°C)±10°C, the hot isostatic pressing pressure is (120MPa-200MPa)±5MPa, and the hot isostatic pressing time is 1h-5h; after completion, the ring sleeve is cooled with the furnace, and the cooling rate is ≤15°C / min;

[0040] S5, machining the cooled ring sheath to remove the ring sheath on the surface to obtain a high-temperature alloy ring blank or a special-shaped ring blank;

[0041] S6, heating and keeping the obtained ring blank, the heating temperature is (1100° C. to 1200° C.) ±10° C., and the keeping time is 1 h to 2 h;

[0042] S7, rolling the heat-insulated ring blank once to obtain a thin-walled ring, designing a corresponding rolling die according to the size, and then fitting the thin-walled ring blank into the rolling die for rotational rolling, wherein the rolling deformation is 10% to 20%, and the rolling strain rate is 0.03s -1 ~0.1s -1 , rolling temperature range is 1000℃~1200℃;

[0043] S8, subjecting the rolled ring to solution + aging heat treatment, wherein the solution temperature is (1000°C to 1200°C) ±10°C, the holding time is 1h to 2h, and air cooling; the aging temperature is (750°C to 900°C) ±10°C, and the holding time is 7h to 8h;

[0044] S9, machining the heat-treated ring to obtain a high-temperature alloy ring of a desired size; see Figure 1 shown.

[0045] Example 1

[0046] This embodiment provides a method for preparing a GH4169 high-temperature alloy ring with a grain size of 7 to 8. The ring has a size of Φ700mm×Φ600mm×100mm. The specific preparation process is as follows:

[0047] S1. The GH4169 high-temperature alloy metal spherical powder was prepared by plasma rotating electrode method with a sieve particle size range of 15 μm to 53 μm and a laser particle size distribution median diameter D50 of 25 μm. Figure 2 As shown, the powder composition meets the GH4169 alloy composition requirements in GB / T14992;

[0048] S2. Use 45 steel to prepare the ring sleeve, the inner cavity of the annular sleeve is 40mm, the outer diameter of the sleeve is 620mm, and the height is 100mm;

[0049] S3. The high-temperature alloy powder is loaded into the designed ring sleeve. After the powder is filled, it is vibrated with a vibration frequency of 30 Hz and an amplitude of 1 mm. The diameter of the 20# steel degassing pipe is Φ8 mm and the length is 1500 mm. The degassing pipe and the sleeve are argon arc welded, and then vacuumed, heated and kept warm. The heating temperature is 450°C and the vacuum degree is 4.2×10 -3 Pa, after keeping warm for 6.5h, the degassing pipeline is clamped and sealed;

[0050] S4, hot isostatic pressing is performed on the powder-filled ring package after the sealing welding in S3, the hot isostatic pressing temperature is 1180℃±10℃, the hot isostatic pressing pressure is 140MPa±5MPa, and the hot isostatic pressing time is 3.5h; after the hot isostatic pressing is completed, it is cooled with the furnace, and the cooling rate is 12℃ / min;

[0051] S5, machining the steel jacket after hot isostatic pressing in S4, completely removing the steel jacket on the surface, and then sandblasting to obtain a high-temperature alloy ring blank, the structure of which after hot isostatic pressing is uniform and has no segregation shrinkage defects;

[0052] S6, heating and keeping the high temperature alloy ring blank in S5, the heating temperature is 1200°C ± 10°C, and the keeping time is 45min ± 10min;

[0053] S7, rolling the high temperature alloy ring blank after heat preservation treatment only once to obtain a high temperature alloy ring, wherein the rolling deformation is 15% and the deformation rate is 0.08s -1 , the pressing temperature is 1000℃, and finally a ring blank of Φ700mm×Φ600mm×100mm is formed;

[0054] S8, performing solution treatment and aging heat treatment on the rolled ring blank, wherein the solution temperature is 1000°C ± 10°C, the holding time is 1h, air cooling, and the aging temperature is 900°C ± 10°C, the holding time is 8h;

[0055] S9, machining the high temperature alloy ring after the treatment in S8 to obtain a high temperature alloy ring with a specification of Φ100mm×Φ50mm×20mm, and its metallographic structure is shown in Figure 3 shown.

[0056] Example 2

[0057] This embodiment provides a method for preparing a GH4169 high-temperature alloy ring with a grain size of 5 to 6. The ring has a size of Φ1100 mm×Φ1050 mm×60 mm. The specific preparation process is as follows:

[0058] S1. The GH4169 high-temperature alloy metal spherical powder was prepared by plasma rotating electrode method with a sieve particle size range of 53 μm to 106 μm and a laser particle size distribution median diameter D50 of 67 μm. Figure 4 As shown, the powder composition meets the GH4169 alloy composition requirements in GB / T14992;

[0059] S2. Use 45 steel to prepare the ring sleeve, the inner cavity of the annular sleeve is 20mm, the outer diameter of the sleeve is 1000mm, and the height is 120mm;

[0060] S3. The high-temperature alloy powder is loaded into the designed ring sleeve. After the powder is filled, it is vibrated with a vibration frequency of 40 Hz and an amplitude of 2 mm. The diameter of the 20# steel degassing pipe is Φ10 mm and the length is 1800 mm. The degassing pipe and the sleeve are argon arc welded, and then vacuumed, heated and kept warm. The heating temperature is 430 °C and the vacuum degree is 3.6×10 -3 Pa, after keeping warm for 5 hours, clamp and seal the degassing pipeline;

[0061] S4, hot isostatic pressing is performed on the powder-filled ring package after the sealing welding in S3, the hot isostatic pressing temperature is 1180℃±10℃, the hot isostatic pressing pressure is 140MPa±5MPa, and the hot isostatic pressing time is 4h; after the hot isostatic pressing is completed, it is cooled with the furnace, and the cooling rate is 10℃ / min;

[0062] S5, machining the steel jacket after hot isostatic pressing in S4, completely removing the steel jacket on the surface, and then sandblasting to obtain a high-temperature alloy ring blank, the structure of which after hot isostatic pressing is uniform and has no segregation shrinkage defects;

[0063] S6, heating and keeping the high temperature alloy ring blank in S5, the heating temperature is 1200°C ± 10°C, and the keeping time is 45min ± 10min;

[0064] S7, rolling the heated and heat-insulated high-temperature alloy ring blank only once to obtain a high-temperature alloy ring, wherein the rolling deformation is 16% and the deformation rate is 0.06s -1 , the pressing temperature is 1100℃, and finally a ring blank of Φ700mm×Φ600mm×100mm is formed;

[0065] S8, performing solution treatment and aging heat treatment on the rolled ring blank, wherein the solution temperature is 1000°C ± 10°C, the holding time is 1h, air cooling, and the aging temperature is 900°C ± 10°C, the holding time is 8h;

[0066] S9, machining the high temperature alloy ring after the treatment in S8 to obtain a high temperature alloy ring with a specification of Φ100mm×Φ50mm×20mm, and its metallographic structure is shown in Figure 5 shown.

[0067] Example 3

[0068] This embodiment provides a method for preparing a GH4169 high-temperature alloy ring with a grain size of 2 to 3. The ring has a size of Φ1500mm×Φ1350mm×40mm. The specific preparation process is as follows:

[0069] S1. The GH4169 high-temperature alloy metal spherical powder was prepared by plasma rotating electrode method with a sieve particle size range of 90 μm to 180 μm and a laser particle size distribution median diameter D50 of 110 μm. Figure 6 As shown, the powder composition meets the GH4169 alloy composition requirements in GB / T14992;

[0070] S2. Use 45 steel to prepare the ring sleeve, the inner cavity of the annular sleeve is 80mm, the outer diameter of the sleeve is 1400mm, and the height is 60mm;

[0071] S3. The high-temperature alloy powder is loaded into the designed ring sleeve. After the powder is filled, it is vibrated with a vibration frequency of 50Hz and an amplitude of 5mm. The diameter of the 20# steel degassing pipe is Φ28mm and the length is 1000mm. The degassing pipe and the sleeve are argon arc welded. Then vacuumization, heating and heat preservation are carried out at 430℃ and the vacuum degree is 3.6×10 -3 Pa, after keeping warm for 5 hours, clamp and seal the degassing pipeline;

[0072] S4, hot isostatic pressing is performed on the powder-filled ring package after the sealing welding in S3, the hot isostatic pressing temperature is 1180℃±10℃, the hot isostatic pressing pressure is 140MPa±5MPa, and the hot isostatic pressing time is 4h; after the hot isostatic pressing is completed, it is cooled with the furnace, and the cooling rate is 15℃ / min;

[0073] S5, machining the steel jacket after hot isostatic pressing in S4, completely removing the steel jacket on the surface, and then sandblasting to obtain a high-temperature alloy ring blank, the structure of which after hot isostatic pressing is uniform and has no segregation shrinkage defects;

[0074] S6, heating and keeping the high temperature alloy ring blank in S5, the heating temperature is 1200°C ± 10°C, and the keeping time is 90min ± 10min;

[0075] S7, rolling the heated and heat-insulated high-temperature alloy ring blank only once to obtain a high-temperature alloy ring, wherein the rolling deformation is 18% and the deformation rate is 0.04s -1 The pressing temperature is 1200℃, and the final ring blank is Φ1540mm×Φ1330mm×45mm;

[0076] S8, performing solution treatment and aging heat treatment on the rolled ring blank, wherein the solution temperature is 1000°C ± 10°C, the holding time is 1h, air cooling, and the aging temperature is 900°C ± 10°C, the holding time is 8h;

[0077] S9, machining the high temperature alloy ring after the treatment in S8 to obtain a high temperature alloy ring with a specification of Φ1500mm×Φ1350mm×40mm, and its metallographic structure is shown in Figure 7 shown.

[0078] The medium particle size of the powder raw materials used in the high temperature alloy rings prepared in Examples 1 to 3, the grain size test after one round of rolling and the 650°C high temperature performance test, the results are shown in Tables 1 and 2 below:

[0079] Table 1 Grain size and forming size of high temperature alloy rings prepared in Examples 1 to 3

[0080]

[0081] Table 2 Grain size and room temperature properties of high temperature alloy rings prepared in Examples 1 to 3

[0082] Example Brand Grain size after rolling and heat treatment Tensile strength / MPa 1 GH4169 7~8 1352 2 GH4169 5~6 1230 3 GH4169 3~4 1123

[0083] Table 1 shows GH4169 rings of different sizes and grain sizes prepared from the same alloy using this method. According to the requirements for grain size, this method can be used to directly prepare them without excessive operations. Table 2 shows the room temperature mechanical properties of rings with different grain sizes. The mechanical properties meet the law of the influence of grain size on mechanical properties. Coarse grains have lower strength and higher plasticity: fine grains have higher strength and lower plasticity. In summary, this method can be used to design product performance in advance, and high-temperature alloy rings of various sizes and grain sizes can be produced. The preparation process is simple and the process is controllable.

[0084] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0085] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a large-sized high-temperature alloy ring with controllable grain size. It is characterized in that The specific steps include: S1. Select high-temperature alloy metal spherical powder with composition and particle size that meet the requirements; S2. After the original formed part size is reduced by 10% to 20% in proportion, the annular cavity thin-walled jacket is designed according to the reduced size, and the jacket shell is spliced ​​and welded according to the designed shape; S3, the powder selected in S1 is loaded into the ring package welded in S2, and after the powder is filled, it is vibrated and compacted, and the package is evacuated and heated and kept warm at the same time, and after the insulation time and vacuum degree meet the requirements at the same time, the package is sealed by welding; S4, hot isostatic pressing the ring sleeve after sealing and welding, and cooling it with the furnace after completion; S5, machining the cooled ring sheath to remove the ring sheath on the surface to obtain a high-temperature alloy ring blank or a special-shaped ring blank; S6, heating and keeping the obtained ring blank warm; S7, rolling the heat-insulated ring blank once to obtain a thin-walled ring, designing a corresponding rolling die according to the size, and then fitting the thin-walled ring blank into the rolling die for rotational rolling; S8, performing solution treatment and aging heat treatment on the ring obtained by rolling; S9. Machining the heat-treated ring to obtain a high-temperature alloy ring of a desired size.

2. The preparation method according to claim 1, It is characterized in that In S1, according to the final grain size requirement, the high-temperature alloy metal spherical powder is screened and the required particle size range is selected, wherein the upper and lower limit difference of the powder screening particle size screen is controlled within 70μm, and the median particle size D50 value of the powder laser particle size is controlled between 10μm and 300μm.

3. The preparation method according to claim 1, It is characterized in that In S2, the annular cavity formed by the sheath has a thickness of 30 mm to 1000 mm, an outer diameter of 50 mm to 1500 mm, and a height of 10 mm to 2000 mm.

4. The preparation method according to claim 1, It is characterized in that In S3, the vibration frequency of the compaction is 30 Hz to 50 Hz, and the amplitude is 1 mm to 5 mm.

5. The preparation method according to claim 1, It is characterized in that In S3, the vacuum degree is ≤3.5×10-3Pa, the jacket heating temperature is 200°C to 500°C, and the insulation time is ≥5h.

6. The preparation method according to claim 1, It is characterized in that In S4, the hot isostatic pressing temperature is 1090° C. to 1410° C., the hot isostatic pressing pressure is 115 MPa to 205 MPa, and the hot isostatic pressing time is 1 h to 5 h.

7. The preparation method according to claim 1, It is characterized in that In S4, the cooling rate is ≤15°C / min.

8. The preparation method according to claim 1, It is characterized in that In S6, the heating temperature is 1090°C to 1210°C, and the insulation time is 1h to 2h.

9. The preparation method according to claim 1, It is characterized in that In S7, the rolling deformation is 10% to 20%, and the rolling strain rate is 0.03s -1 ~0.1s -1 , the rolling temperature range is 1000℃~1200℃.

10. The preparation method according to claim 1, It is characterized in that In S8, the solution temperature is 990°C to 1210°C, the holding time is 1h to 2h, and air cooling is performed; the aging temperature is 740°C to 910°C, and the holding time is 7h to 8h.

Citation Information

Patent Citations

  • Ti2AlNb alloy plate as well as preparation method and application thereof

    CN115971492A

  • Preparation method and application of high-temperature alloy ring piece with short process and high material utilization rate

    CN117206527A

  • Preparation method of large-specification titanium alloy ring material

    CN117259760A

  • Preparation method of tungsten particle reinforced amorphous matrix composites

    US20190232366A1

  • Hot isostatic pressing process for ti 2alnb alloy powder

    WO2021031231A1

Cited By

  • Preparation method of short-process Inconel 718 alloy ring piece

    CN120243857A

  • A short-process preparation method for Inconel 718 alloy rings

    CN120243857B

  • Preparation method and application of large-size titanium steel bimetallic ring piece

    CN120838968A

  • Preparation method and application of large-size titanium steel bimetallic ring piece

    CN120838968B