Method for joining dissimilar metal bodies and hot forging die
Through solid solution process and solid phase diffusion bonding technology, the heat treatment of different metal bodies is optimized, which solves the problems of high heat treatment costs and short mold life in the prior art, and achieves more efficient metal characteristics and life extension.
Patent Information
- Application Number
- CN202410310656.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-03-19
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot fully utilize the characteristics of metal materials in the heat treatment of different metal bodies, and the cost and energy of bonding and heat treatment are high, resulting in a short life of the hot forging mold and increasing waste generation.
Through the solid solution process, the precipitated hardened heat-resistant steel is heated to high temperature and quenched, and then solid phase diffusion bonding and aging treatment with the hot working tool steel, quenching and tempering, reducing the number of heat treatments, and optimizing the hardness and durability of the metal body.
It effectively reduces the cost and energy of bonding and heat treatment, extends the life of the hot forging mold, appropriately exerts the characteristics of different metal bodies, and reduces waste generation.
Smart Images

Figure CN118989546A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for joining dissimilar metal bodies, in which a second metal body made of precipitation-hardened heat-resistant steel is joined to a first metal body made of hot-working tool steel, and a hot forging die manufactured using the joining method. Background Art
[0002] In recent years, efforts have been actively made to significantly reduce the generation of waste through prevention, reduction, recycling and reuse of waste. To achieve this, research and development related to the reuse of metal materials is being carried out.
[0003] In the past, the crankshaft of the internal combustion engine was formed by hot forging. Hot forging is a processing method that uses a die to repeatedly apply a high pressure load to a structural material that has been heated to a high temperature to reduce its deformation resistance to transfer the shape of the die. The die slides repeatedly with the structural material under high temperature and high pressure, so the life of the die is short. If the life of the die is short, not only does it need to be regenerated by mechanical processing of the die surface, but the production cost of the die also increases. In addition, various losses occur, such as the need to stop the operation of the production line in order to replace the die, and the need to adjust various conditions based on wear.
[0004] In order to suppress the wear caused by sliding and achieve a longer service life, it is considered to manufacture the mold with a composite metal. Patent document 1 discloses a composite mold for hot forging, which has a first weld overlay layer composed of an alloy that emphasizes high-temperature wear resistance and a second weld overlay layer composed of an alloy that emphasizes high-temperature strength. The mold has a burr flow promotion area that promotes the flow of burrs (burrs) from the rough material that becomes a forged product and a burr flow suppression area that suppresses the flow of burrs from the rough material. The first weld overlay layer that emphasizes high-temperature wear resistance is welded in the burr flow promotion area, and the second weld overlay layer that emphasizes high-temperature strength is welded in the burr flow suppression area.
[0005] In addition, Patent Document 2 discloses a heat treatment method for joining a first metal material (Inconel 718) composed of a precipitation hardening heat-resistant alloy and a second metal material (3Cr-Mo-V steel) composed of a non-precipitation hardening alloy. In this heat treatment method, the hardness of the hardness reduction area of the first metal material caused by the thermal effect accompanying the joining and the hardness increase area of the second metal material caused by the thermal effect are restored. Specifically, first, a heat treatment is performed within a range where the solid solution (solution) heat treatment conditions of the first metal material and the quenching treatment conditions of the second metal material overlap (900°C to 1200°C / 0.1h or more). As a result, the hardness of the area of the first metal material whose hardness is reduced due to joining is restored to the high hardness side. Then, a secondary heat treatment is performed within a range where the aging treatment conditions of the first metal material and the tempering treatment conditions of the second metal material overlap (470°C to 850°C / 0.1h or more). As a result, the hardness of the area of the second metal material whose hardness is increased due to joining is restored to the low hardness side.
[0006] [Prior art literature]
[0007] [Patent Document]
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 11-347678
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 10-298663 Summary of the invention
[0010] [Problems to be Solved by the Invention]
[0011] However, in the technology of patent document 1, the first overlay layer and the second overlay layer joined by overlay welding are not subjected to heat treatment after joining, so the characteristics of these metal materials cannot be fully utilized. In addition, the technology of patent document 2 cannot be applied to the case where the solid solution (solution) heat treatment conditions of the first metal material and the quenching treatment conditions of the second metal material are not repeated, and the aging treatment conditions of the first metal material and the tempering treatment conditions of the second metal material are not repeated. Even in the case of repeated heat treatment conditions, since the two metal materials are heat treated at the same time, it is impossible to heat treat them under the conditions that are most suitable for the two metals. In this way, in the technology related to the dissimilar metal body containing dissimilar metal materials, there is room for improvement in properly exerting the characteristics of each metal material.
[0012] In addition, the technology of Patent Document 2 applies the heat treatment method to dissimilar metal bodies joined by any one of arc welding, friction welding, and liquid phase diffusion bonding. However, in the case where the dissimilar metal bodies are formed by joining two metal bodies by solid phase diffusion bonding, if the dissimilar metal bodies are rapidly cooled in a heat treatment after joining, cooling cracks may occur due to thermal stress during cooling, phase change stress, difference in thermal expansion coefficient between dissimilar metals, heat transfer at the bonding interface, etc.
[0013] Here, it is considered that after the first metal material composed of the precipitation hardening heat-resistant alloy is subjected to solution treatment and aging treatment, the first metal material and the second metal material are joined to each other by solid phase diffusion bonding. However, in this case, after the three heat treatments for solution treatment, aging treatment and solid phase diffusion bonding, two more heat treatments are required for quenching and tempering of the second metal material composed of the non-precipitation hardening alloy. Therefore, the cost and energy required for bonding and heat treatment are large.
[0014] In view of the above background, the present invention aims to appropriately utilize the characteristics of the metal materials contained in the dissimilar metal bodies and reduce the cost and energy required for joining and heat treatment. In addition, the life of the hot forging die is further extended, which helps to significantly reduce the generation of waste.
[0015] [Methods for solving the problem]
[0016] In order to solve the above-mentioned problems, one embodiment of the present invention is a method for joining dissimilar metal bodies 2 and 3, wherein the dissimilar metal bodies 2 and 3 are formed by joining a second metal body 17 composed of precipitation hardening type heat-resistant steel and a first metal body 16 composed of hot working tool steel, comprising: a solution treatment process, heating the second metal body to a first specified temperature T1 higher than the solution temperature (e.g., 965°C) of the precipitation hardening type heat-resistant steel, so that the second metal body is dissolved, and then rapidly cooling the second metal body to precipitation harden the second metal body; and a joining / aging process, after the solution treatment process, heating the second metal body to a temperature lower than the solution temperature of the precipitation hardening type heat-resistant steel and higher than the precipitation hardening temperature while keeping the second metal body in close contact with each other at a specified pressure. A second prescribed temperature T2 which is higher than the aging temperature of the precipitation hardening type heat-resistant steel, by maintaining the second prescribed temperature for a prescribed time corresponding to the second prescribed temperature, solid phase diffusion bonding the second metal body to the first metal body, and aging treatment the second metal body; a quenching process, after the bonding / aging process, heating the dissimilar metal body formed by bonding the first metal body to the second metal body to a third prescribed temperature T3 which is lower than the solid solution temperature of the precipitation hardening type heat-resistant steel and higher than the quenching temperature of the hot working tool steel, and then cooling, thereby quenching the first metal body; and a tempering process, after the quenching process, heating the dissimilar metal body to the tempering temperature of the hot working tool steel which is lower than the quenching temperature.
[0017] According to this method, the solutionizing process of the second metal body is performed before the solid phase diffusion bonding, so that the second metal body can be reliably precipitated and hardened without being restricted by temperature and cooling rate. In addition, since the solid phase diffusion bonding and aging treatment are performed at the same time, the heat treatment only needs to be performed 4 times. Therefore, the cost and energy required for bonding and heat treatment can be reduced. In the quenching process and tempering process of the first metal body, the first metal body can be quenched and tempered without re-solidifying the second metal body and without generating cooling cracks.
[0018] In the above method, the third specified temperature when quenching the first metal body in the quenching process may be in a temperature range above 950°C and lower than 1100°C, and the precipitation-hardened heat-resistant steel is a precipitation-hardened Ni-based alloy that does not undergo solid solution at a temperature lower than 950°C but undergoes solid solution at a temperature lower than 1100°C.
[0019] According to this aspect, the first metal body can be quenched without coarsening, and the characteristics of the hot working tool steel and precipitation hardening heat resistant steel of the dissimilar metal body including the precipitation hardening Ni-based alloy can be appropriately exhibited.
[0020] Preferably, the first predetermined temperature in the solution treatment step is higher than a coarsening temperature of the hot working tool steel.
[0021] According to this method, precipitation hardening type heat-resistant steel with high heat resistance and wear resistance can be used, which can reliably precipitate harden the second metal body in the solutionizing process, or has a high solutionizing temperature and requires rapid cooling such as water cooling during solutionizing. As a result, the durability of the dissimilar metal body is improved.
[0022] In the above method, it may be that, in the quenching process, the time for maintaining the third specified temperature is estimated to be the estimated minimum time required for the entire first metal body to reach the third specified temperature based on the size of the first metal body, and the dissimilar metal body is immediately cooled after the estimated minimum time has passed.
[0023] According to this aspect, the first metal body can be quenched without overaging the second metal body made of precipitation-hardening heat-resistant steel.
[0024] In the above aspect, in the solution treatment step, the second metal body may be cooled by water cooling.
[0025] According to this aspect, the solute atoms of the precipitation-hardening heat-resistant steel can be reliably precipitated to harden the second metal body. In addition, the first metal body is quenched by cooling, but is annealed by heating and maintaining it at the aging temperature in the aging process.
[0026] In the above aspect, in the quenching step, the dissimilar metal body may be cooled by air cooling or oil cooling.
[0027] If the first metal body made of hot working tool steel is cooled by water cooling, there is a possibility that cracks will be generated in the first metal body due to thermal stress. According to this aspect, the first metal body can be quenched without generating cracks.
[0028] In the above aspect, the quenching step and the joining / aging step may be performed continuously.
[0029] According to this embodiment, the number of heat treatments can be reduced from four to three.
[0030] In the above aspect, the first metal body and the second metal body may each have a hardness of HRC38 or more and HRC47 or less after the tempering step.
[0031] According to this aspect, the first metal body and the second metal body can be made to have a hardness suitable for a hot forging die.
[0032] The hot working tool steel may be SKD61, and the precipitation hardening heat-resistant steel may be NCF 750.
[0033] According to this embodiment, it is possible to manufacture a dissimilar metal body using SKD61 and NCF750 and appropriately utilizing their characteristics.
[0034] In addition, in order to solve the above-mentioned problems, one embodiment of the present invention is a hot forging mold 1, which has a lower mold 2 and an upper mold 3, and the lower mold 2 and the upper mold 3 are formed by the dissimilar metal bodies formed by joining the second metal body to the first metal body by the above-mentioned joining method, wherein the lower mold and the upper mold have: cavities 8, 9, which are recessed in their respective parting surfaces 6, 7; and inclined surfaces 12, 13, which are formed on the outside of the cavities in order to suppress burrs 5 generated between the parting surfaces, the mold bodies of the lower mold and the upper mold are both formed by the first metal body, and the inclined surfaces of the lower mold and the upper mold are both formed by the second metal body.
[0035] According to this method, the life of the hot forging die is extended by providing the second metal body having high heat resistance and wear resistance on the inclined surface that functions as the burr suppression portion. In addition, precipitation hardening heat-resistant steel is very expensive compared to hot working tool steel, but since the second metal body composed of precipitation hardening heat-resistant steel is partially provided on the upper die and the lower die, the increase in the material cost of the hot forging die is suppressed.
[0036] [Effects of the invention]
[0037] According to the above aspect, the characteristics of the metal material included in the dissimilar metal body can be appropriately utilized, and the cost and energy required for joining and heat treatment can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a cross-sectional view of a hot forging die according to an embodiment.
[0039] Figure 2 It is a timing chart showing the general thermal process of (A) hot work tool steel, (B) precipitation hardening heat-resistant steel, and (C) solid phase diffusion bonding.
[0040] Figure 3 It is a timing chart showing the steps of joining and heat treating dissimilar metal bodies according to the embodiment.
[0041] Description of Reference Numerals
[0042] 1: Hot forging die
[0043] 2: Lower mold
[0044] 3: Upper mold
[0045] 4: Roughly formed product
[0046] 5: Burr
[0047] 6: Parting surface
[0048] 7: Parting surface
[0049] 8: Cavity
[0050] 9: Cavity
[0051] 10: Burr runner
[0052] 11: Burr runner
[0053] 12: Inclined surface
[0054] 13: Inclined surface
[0055] 16: First metal body
[0056] 17: Second metal body
[0057] T1: The first specified temperature
[0058] T2: The second specified temperature
[0059] T3: The third specified temperature DETAILED DESCRIPTION
[0060] Figure 1 1 is a cross-sectional view of a hot forging die 1 according to an embodiment. Figure 1 As shown, the hot forging die 1 includes a lower die 2 and an upper die 3 constituting a forging die as a composite die. The hot forging die 1 is a rough-work forming die for rough-working a rough-formed product 4 obtained by crushing a raw material of a carbon steel system heated to a high temperature by hot working. The hot forging die 1 is not used to form shaft parts with simple shapes such as drive shafts, but is used to form rough-worked forgings of special-shaped parts with complex shapes. In the present embodiment, the hot forging die 1 forms a rough-worked forging of a crankshaft of an internal combustion engine. In addition, the rough-worked forging formed by the hot forging die 1 is subjected to a second rough-working forming treatment if necessary, and then subjected to a finishing treatment, a trimming treatment, etc. to form a final formed product.
[0061] The lower die 2 has a horizontally extending upward parting surface 6, and the upper die 3 has a corresponding downward parting surface 7. The parting surface 6 of the lower die 2 and the parting surface 7 of the upper die 3 are respectively provided with cavities 8 and 9 corresponding to the contour of the rough forged product of the crankshaft. The part of the parting surface 6 and 7 near the cavities 8 and 9 is a burr flow channel 10 and 11 for the burr 5 (burr) to which a high pressure is applied to slide when a part of the rough-formed product 4 flows out to the side between the two cavities 8 and 9 and becomes a burr 5 (burr). The burr flow channels 10 and 11 of the lower die 2 and the upper die 3 are highly parallel and extend horizontally.
[0062] On the outside of the two burr channels 10, 11, inclined surfaces 12, 13 are provided which are parallel to each other and are inclined relative to the burr channels 10, 11. The inclined surfaces 12, 13 are inclined downward toward the outside. During forging, these inclined surfaces 12, 13 suppress the expansion of the burr 5 which slides between the burr channels 10, 11 while being held at high pressure by the burr channels 10, 11. Thus, the filling of the rough formed product 4 into the cavity 8, 9 is promoted. That is, the inclined surfaces 12, 13 are burr suppression parts which suppress the burr 5 generated between the burr channels 10, 11 of the parting surfaces 6, 7.
[0063] The lower mold 2 and the upper mold 3 are respectively heterogeneous metal bodies formed of heterogeneous metals. Specifically, the lower mold 2 and the upper mold 3 have a first metal body 16 composed of hot working tool steel constituting the majority thereof and a second metal body 17 composed of hardened heat-resistant steel joined to the first metal body 16. The first metal body 16 constitutes the mold body of the lower mold 2 and the upper mold 3.
[0064] The second metal body 17 is formed in a plate shape to form the outer portion of the burr flow paths 10 and 11 and the inclined surfaces 12 and 13 in the parting surfaces 6 and 7 of the lower mold 2 and the upper mold 3, and is joined to the first metal body 16 by solid phase diffusion bonding. Since the second metal body 17 is not provided on the inner portion of the burr flow paths 10 and 11, it is not necessary to form the second metal body 17 in a complex shape along the contour of the rough formed product 4 of the crankshaft.
[0065] The second metal body 17 is made of hot working tool steel, and thus has higher heat resistance and wear resistance than the first metal body 16. Thus, by providing the second metal body 17 on the inclined surfaces 12 and 13 that function as burr suppression portions, the life of the hot forging die 1 is extended. In addition, precipitation hardening heat-resistant steel is very expensive compared to hot working tool steel, but the second metal body 17 made of precipitation hardening heat-resistant steel is partially provided on the lower die 2 and the upper die 3, so that the increase in the material cost of the hot forging die 1 can be suppressed.
[0066] The first metal body 16 can be composed of a metal material (first metal material) having high heat resistance and wear resistance and excellent toughness among hot working tool steels, and is formed of SKD61 in this embodiment. SKD61 is an alloy steel for hot molds specified in JIS G 4404:2015 alloy tool steel. The heat treatment temperature, cooling method, hardness, etc. of SKD61 are specified in JIS. The quenching of SKD61 is specified to be 1020°C and air cooling, and the tempering of SKD61 is specified to be 550°C and air cooling. However, the quenching temperature and tempering temperature of SKD61 are not limited to this, and can be set to an appropriate temperature to exert appropriate hardness, toughness and other characteristics consistent with the purpose of the first metal body 16.
[0067] Figure 2 1 is a timing chart showing the general heat treatment process of (A) hot work tool steel and (B) precipitation hardening heat resistant steel. Figure 2 As shown in (A), SKD61 as a hot work tool steel is heated to 1020° C., for example, and then cooled by air cooling to be quenched (quenching process), and then heated to 650° C. to be tempered (tempering process).
[0068] In JIS G 4404, the quenching and tempering hardness of SKD61 is specified as HV (Vickers hardness) 513. It should be noted that HV 513 can be converted to HRC (Rockwell C hardness) 50. In addition, the annealing temperature of SKD61 is specified as 820-870°C, and the annealing hardness is specified as HBW (HBW is Brinell hardness (10 mm ball load 29.4 kN)) 229 or less.
[0069] The coarsening temperature of SKD61 is 1100°C. If SKD61 is heated to 1100°C or higher during quenching, the SKD61 will coarsen and the toughness after quenching and tempering will decrease. That is, the first metal body 16 composed of SKD61 becomes brittle and is not suitable for a forging die body that generates high pressure. Therefore, the quenching of SKD61 needs to be performed at a temperature lower than 1100°C.
[0070] On the other hand, the inventors have confirmed through experiments that even if SKD61 is not heated to 1020°C specified in JIS, as long as it is heated to a specified quenching temperature or above, the specified hardness can be obtained after quenching and tempering. Here, the specified hardness can be a hardness sufficient for forging rough parts of special-shaped parts, that is, HRC38 or above, and more preferably HRC41 or above. Specifically, the inventors have confirmed through experiments that by heating SKD61 to 950°C or above, the hardness of SKD61 after quenching and tempering is HRC38 or above, and more specifically, HRC41 or above.
[0071] That is, during quenching, SKD61 is preferably heated to a temperature not less than the quenching temperature of 950° C. and lower than the coarsening temperature of 1100° C. In the present embodiment, as described later, NCF 750 is solutionized at 965° C., so during quenching, SKD61 is preferably heated to a temperature not less than 950° C. and lower than 965° C.
[0072] The second metal body 17 can be made of a metal material (second metal material) having higher heat resistance and wear resistance and excellent toughness than the metal material of the first metal body 16, and in this embodiment, is made of NCF 750. NCF 750 is a superalloy steel specified in JIS G 4901 Corrosion-resistant and heat-resistant superalloy rods and 4902 Corrosion-resistant and heat-resistant superalloy plates: 2019.
[0073] In addition, Appendix A (reference) of JIS G 4902 describes an example of heat treatment conditions for NCF 750. As a solution heat treatment of NCF 750, (S1) rapid cooling at 1135-1165°C and (S2) rapid cooling at 965-995°C are described. In addition, as an aging treatment of NCF 750, it is described that (H1) after S1 solution treatment, it is kept at 800-830°C for 24 hours, air-cooled to room temperature, and kept at 690-720°C for 20 hours and then rapidly cooled. Furthermore, as an aging treatment, it is described that (H2) after S2 solution heat treatment, it is kept at 720-740°C for 8 hours, furnace-cooled to 610-630°C, and then aged at this temperature and air-cooled, with a total aging time of 18 hours. However, the solution treatment temperature and aging treatment temperature of NCF 750 are not limited thereto, and may be set to appropriate temperatures so as to exhibit appropriate properties such as hardness and toughness in accordance with the purpose of the second metal body 17 .
[0074] As metal materials of NCF 750 standard, there are DSALOY (registered trademark) X-750 of Daido Steel Co., Ltd., Inconel (registered trademark) X 750 made by Special Metal Co., Ltd., etc. These are precipitation hardening type Ni-based alloys. The second metal body 17 can also be formed by DSA 760 of Daido Steel Co., Ltd., which is a Ni-based alloy and has excellent high-temperature wear resistance and corrosion resistance, instead of NCF 750.
[0075] like Figure 2 As shown in (B), NCF 750, which is a precipitation hardening heat-resistant steel, is heat treated according to the above (H1). For example, NCF 750 is heated to 1150°C, and then rapidly cooled by water cooling (W / C) to perform a solution treatment (solution treatment process), and then heated to 850°C and maintained for 16 hours to perform an aging treatment (aging process).
[0076] In JIS G 4902, the hardness of NCF 750 is specified for each heat treatment (applicable to thickness exceeding 0.6 mm and below 6 mm). When only solution heat treatment (S1) or (S2) is performed, the hardness of NCF 750 is specified to be HBW 321 or less, HRC 35 or less, and HV 335 or less. In the case of aging treatment after solution heat treatment (H1), the hardness of NCF 750 is specified to be HBW 262 or more, HRC 26 or more, and HV 270 or more. In the case of aging treatment after solution heat treatment (H2), the hardness of NCF 750 is specified to be HBW 302-363, HRC 32-40, and HV 313-382.
[0077] In this embodiment, NCF750 is used for the rough forging die of the special-shaped component as described above. Therefore, the hardness of NCF750 is preferably HRC38 or more, and more preferably HRC41 or more.
[0078] In this embodiment, the second metal body 17 composed of NCF 750 and the first metal body 16 composed of SKD61 are joined by solid phase diffusion bonding. Solid phase diffusion bonding is a bonding performed at a temperature below the melting point of the base material. It is a method in which the base materials are brought into close contact, pressurized in a manner that causes as little plastic deformation as possible under temperature conditions below the melting point of the base materials, and bonded by diffusion of atoms generated between the bonding surfaces. In solid phase diffusion bonding, the base materials that are in close contact with each other are heated and pressurized in an atmosphere controlled so that the bonding surfaces are not oxidized, and bonding is performed by diffusion of atoms.
[0079] like Figure 2 As shown in (C), in solid-phase diffusion bonding, the second metal body 17 and the first metal body 16 are pressurized to make them close to each other, and then heated to a temperature below the melting point of SKD61 and NCF 750 (for example, 1050°C), and the pressurized state and temperature are maintained for a specified time determined by the temperature (for example, 4 hours in the case of 1050°C). As a result, atoms diffuse between the bonding surfaces, and the second metal body 17 and the first metal body 16 are bonded to each other (bonding process). In solid-phase diffusion bonding, the higher the temperature, the shorter the holding time. As shown by the imaginary line in the figure, the lower the temperature, the longer the holding time is required.
[0080] Next, the manufacturing method of the hot forging die 1 thus constructed will be described. It should be noted that both the lower die 2 and the upper die 3 are made of dissimilar metal bodies and their manufacturing methods are the same. Hereinafter, they will be referred to as dissimilar metal bodies for description.
[0081] Figure 3 It is a timing diagram showing the process of joining and heat treatment of dissimilar metal bodies in an embodiment. As shown in the figure, first, only the second metal body 17 is subjected to a solution treatment. Specifically, the second metal body 17 is arranged in a furnace and heated to 1150°C. After the second metal body 17 is dissolved, the dissimilar metal body is quenched by water cooling to precipitate and harden the second metal body 17 (solution treatment process). The 1150°C is a first prescribed temperature T1 that is higher than the solution temperature of NCF 750. As mentioned above, the minimum temperature of the solution heat treatment of NCF 750 recorded in JIS is 965°C (S2), and 1150°C is higher than it, and higher than 1035°C (S2).
[0082] The first predetermined temperature T1 is preferably a temperature higher than the coarsening temperature of SKD61, which is 1100°C. Thus, the second metal body 17 is reliably precipitated and hardened in the solutionizing process. Alternatively, other precipitation hardening heat-resistant steels having a higher solutionizing temperature than NCF 750 and requiring rapid cooling such as water cooling during solutionizing and having higher heat resistance and wear resistance can be used. Thus, the durability of the dissimilar metal body is improved.
[0083] In the solution treatment step, the second metal body 17 is cooled by water cooling, so that the solute atoms of the NCF 750 are reliably precipitated and the second metal body 17 is hardened.
[0084] Next, the second metal body 17 and the first metal body 16 constituting the mold body are arranged in a furnace for solid phase diffusion bonding, heated to 900°C in a state of being in close contact with each other at a specified pressure, and the pressurized state and 900°C are maintained for 16 hours. 900°C is a second specified temperature T2 which is lower than the solution temperature of NCF 750 and higher than the aging temperature of NCF 750. As mentioned above, the minimum temperature of the solution heat treatment of NCF 750 recorded in JIS is 965°C (S2), and the minimum temperature of the aging temperature is 720°C (H2). That is, the second specified temperature T2 is set to 900°C which is lower than 965°C and higher than 720°C. 16 hours is the time required to perform aging treatment on the second metal body 17 at 900°C and solid phase diffusion bonding of the second metal body 17 and the first metal body 16 at 900°C. Thus, the second metal body 17 is solid-phase diffusion-bonded to the first metal body 16, and the second metal body 17 is subjected to aging treatment (bonding / aging process). Through this bonding treatment, a dissimilar metal body is obtained in which the first metal body 16 made of hot working tool steel is bonded to the second metal body 17 made of precipitation hardening heat-resistant steel. After the bonding / aging treatment, the dissimilar metal body is taken out of the furnace.
[0085] Then, after the dissimilar metal body is arranged in a furnace and heated to 950°C, the dissimilar metal body is cooled by air cooling or oil cooling, and the first metal body 16 is quenched (quenching process). This 950°C is higher than the aging temperature of NCF 750, and is the third prescribed temperature T3 above the quenching temperature of SKD61 quenching (as mentioned above, the hardness of SKD61 after quenching and tempering is HRC38 or above, more specifically, the temperature of HRC41 or above). In addition, the third prescribed temperature T3 (950°C) needs to be lower than the solution temperature of NCF750. The inventors of the present invention have confirmed that the minimum value of the solution temperature of NCF 750 recorded in JIS G 4902 is 965°C, and 950°C is lower than it, so that NCF 750 is not dissolved, that is, 950°C is lower than the solution temperature of NCF 750.
[0086] After the quenching process, the dissimilar metal body is heated to 550°C for tempering (tempering process). The 550°C is the tempering temperature of SKD61, which is lower than the quenching temperature of SKD61. Thereafter, the dissimilar metal body is cooled to complete the manufacture of the dissimilar metal body, that is, the lower mold 2 or the upper mold 3.
[0087] The lower die 2 or the upper die 3 is manufactured in this manner, and the hardness of each of the first metal body 16 and the second metal body 17 after the tempering process is HRC38 or more and HRC47 or less, which is a hardness suitable for the hot forging die 1. The hardness of each of the first metal body 16 and the second metal body 17 after the tempering process is preferably HRC41 or more and HRC43 or less.
[0088] Thus, in the method for joining dissimilar metal bodies, the second metal body 17 is first subjected to a solid solution treatment process, and then the second metal body 17 is simultaneously subjected to solid phase diffusion bonding with the first metal body 16 and aging treatment of the second metal body 17. That is, the solid solution treatment process of the second metal body 17 is performed before solid phase diffusion bonding, so that the second metal body 17 is not restricted by the temperature and cooling rate of SKD61, and the second metal body 17 can be reliably precipitated and hardened. In addition, since solid phase diffusion bonding and aging treatment are performed simultaneously, Figure 3 As shown in FIG. 1 , the heat treatment which normally requires five times can be reduced to four times. Therefore, the cost and energy required for the joining and heat treatment can be reduced.
[0089] In addition, in this joining method, after the joining / aging step, a quenching step of heating the dissimilar metal body to 950° C. and then cooling is performed, and then a tempering step of heating the dissimilar metal body to 550° C. is performed. Thus, in the quenching step, the second metal body 17 is not solid-dissolved, the first metal body 16 is quenched, and in the tempering step, the first metal body 16 is tempered. Through these steps, the characteristics of the hot working tool steel and the precipitation hardening type heat-resistant steel contained in the dissimilar metal body can be appropriately exerted.
[0090] Thus, the third predetermined temperature T3 when the first metal body 16 is quenched in the quenching process is in the temperature range of 950°C or more and lower than 1100°C, so that the first metal body 16 composed of SKD61 is quenched without coarsening. In addition, since NCF 750 (precipitation hardening heat-resistant steel) forming the second metal body 17 is a precipitation hardening Ni-based alloy that does not dissolve at a temperature lower than the quenching temperature, 950°C, but dissolves at a temperature lower than 1100°C, the characteristics of the hot working tool steel and precipitation hardening heat-resistant steel contained in the dissimilar metal body can be appropriately exerted.
[0091] In the quenching process, the time for which the dissimilar metal body is kept at 950°C (the third predetermined temperature T3) is the estimated minimum time required for the entire first metal body 16 to reach 950°C based on the size of the first metal body 16, and the dissimilar metal body is immediately cooled after the estimated minimum time has passed. As a result, the second metal body 17 composed of NCF 750 (precipitation hardening heat-resistant steel) will not become over-aged, and the first metal body 16 is quenched.
[0092] If the first metal body 16 made of hot working tool steel is cooled by water cooling in the quenching process, thermal stress may cause cracks in the first metal body 16. In this embodiment, the dissimilar metal body is cooled by air cooling, so that the first metal body 16 is quenched without cracks.
[0093] Furthermore, by using SKD61 as the hot work tool steel for the first metal body 16 and using NCF750 as the precipitation hardening heat-resistant steel for the second metal body 17, dissimilar metal bodies that appropriately exhibit their characteristics are manufactured.
[0094] The above is the end of the description of the specific embodiment, but the present invention is not limited to the above embodiment and modification examples, and can be widely modified. Figure 3 As shown by the imaginary line in the middle, the tempering process can also be performed continuously with the joining / aging process, that is, without cooling the dissimilar metal body. In this case, the time from the moment when the dissimilar metal body is set to 900°C to the moment when the temperature rise for quenching begins can be 9 hours. By this method, the heat treatment can be reduced from 4 times to 3 times.
[0095] In addition, the shape of the hot forging die 1 is not limited thereto, and the dissimilar metal body can also be used for dies other than the hot forging die 1, and tools other than the die. In addition, the specific structure, arrangement, quantity, raw materials, specific steps, temperature, time, etc. of each component and part can be appropriately changed as long as they do not deviate from the scope of the present invention. In addition, not all of the components shown in the above embodiment are required, and they can be appropriately selected.
Claims
1. A method for joining dissimilar metal bodies, wherein the dissimilar metal bodies are formed by joining a second metal body made of precipitation hardening heat-resistant steel to a first metal body made of hot working tool steel, wherein: The joining method includes: A solution treatment step of heating the second metal body to a first predetermined temperature higher than the solution temperature of the precipitation hardening heat-resistant steel to dissolve the second metal body, and then rapidly cooling the second metal body to precipitation harden the second metal body; a bonding / aging step, after the solution treatment step, heating the second metal body and the first metal body to a second predetermined temperature lower than the solution temperature of the precipitation hardening heat-resistant steel and higher than the aging temperature of the precipitation hardening heat-resistant steel in a state where the second metal body and the first metal body are in close contact with each other at a predetermined pressure, and performing solid phase diffusion bonding on the second metal body and performing aging treatment on the second metal body by maintaining the second predetermined temperature for a predetermined time corresponding to the second predetermined temperature; a quenching step of, after the joining / aging step, heating the dissimilar metal body formed by joining the second metal body to the first metal body to a third predetermined temperature that is lower than the solution temperature of the precipitation hardening heat-resistant steel and higher than the quenching temperature of the hot working tool steel, and then cooling the dissimilar metal body to quench the first metal body; and A tempering step, after the quenching step, of heating the dissimilar metal body to a tempering temperature of the hot working tool steel that is lower than the quenching temperature.
2. The method for joining dissimilar metal bodies according to claim 1, wherein: The third predetermined temperature when quenching the first metal body in the quenching step is in a temperature range of 950° C. or higher and lower than 1100° C., The precipitation hardening heat-resistant steel is a precipitation hardening Ni-based alloy that does not undergo solid solution at a temperature lower than 950°C but undergoes solid solution at a temperature lower than 1100°C.
3. The method for joining dissimilar metal bodies according to claim 2, wherein: The first predetermined temperature in the solution treatment step is higher than a coarsening temperature of the hot work tool steel.
4. The method for joining dissimilar metal bodies according to any one of claims 1 to 3, wherein: In the quenching process, the time for maintaining the third specified temperature is estimated to be the estimated minimum time required for the entire first metal body to reach the third specified temperature based on the size of the first metal body, and the dissimilar metal body is immediately cooled after the estimated minimum time.
5. The method for joining dissimilar metal bodies according to any one of claims 1 to 3, wherein: In the solution treatment step, the second metal body is cooled by water cooling.
6. The method for joining dissimilar metal bodies according to any one of claims 1 to 3, wherein: In the quenching step, the dissimilar metal body is cooled by air cooling or oil cooling.
7. The method for joining dissimilar metal bodies according to any one of claims 1 to 3, wherein: The quenching step and the joining / aging step are performed continuously.
8. The method for joining dissimilar metal bodies according to any one of claims 1 to 3, wherein: After the tempering step, the first metal body and the second metal body each have a hardness of HRC 38 or more and HRC 47 or less.
9. The method for joining dissimilar metal bodies according to any one of claims 1 to 3, wherein: The hot working tool steel is SKD61, and the precipitation hardening heat-resistant steel is NCF 750.
10. A hot forging die, comprising a lower die and an upper die, wherein the lower die and the upper die are formed by the dissimilar metal bodies formed by joining the second metal body to the first metal body by the joining method according to claim 1, wherein: The lower mold and the upper mold have cavities recessed in their respective parting surfaces and inclined surfaces formed on the outer sides of the cavities to suppress burrs generated between the parting surfaces. The mold bodies of the lower mold and the upper mold are both formed by the first metal body. The inclined surfaces of the lower mold and the upper mold are both formed by the second metal body.