Flat composite brazing filler metal and preparation method and application thereof
By setting through holes on the flat composite solder and embedding high melting point metal balls, the problems of high void rate and poor thickness uniformity of the welding layer are solved, and the high quality of the welding layer and the reliability of components are improved.
Patent Information
- Application Number
- CN202411106958.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
Smart Images

Figure CN118989716A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solder, and in particular to a flat composite solder and a preparation method and application thereof. Background Art
[0002] Welding is a method of connecting two electronic components by heating the solder to a temperature lower than the melting point of the two electronic components to be connected but higher than the melting point of the solder. During service, the solder layer between electronic components will be subjected to severe tests such as thermal stress, high-density current and power cycle. As electronic components become more sophisticated and integrated, the requirements for the quality of the solder layer are getting higher and higher. The solder void rate and thickness uniformity of the solder layer will affect the quality of the solder layer. If the solder void rate of the solder layer is too large or the thickness uniformity is not good, the reliability of the solder joint will decrease, the resistance to cold and hot cycles and impact resistance will deteriorate, the solder layer will be prone to cracks or even breakage, and it is very likely to cause irreparable damage to the components.
[0003] At present, soldering is generally performed by reduction soldering with auxiliary agents, such as flux, formic acid or hydrogen. During welding, the auxiliary agent itself or the auxiliary agent reduces the oxide film on the surface of the solder and the solder surface, which will generate gas. The gas generated during welding is enclosed in the soldering surface due to the lack of discharge channels, which is inconvenient to discharge or even impossible to discharge, thus bringing a lot of troubles to reducing the soldering void rate and improving the soldering quality. At the same time, since the solder is in a fluid state after melting, it has no supporting capacity. During the welding process, the direction of the pressure on the soldering surface of the upper and lower electronic components is poorly perpendicular to the soldering surface, which will cause the soldering layer to tilt, and then cause the thickness of the soldering layer to be uneven. In the thicker part of the soldering layer, the thermal resistance of the soldering layer is larger, so the heat generated by the electronic components will accumulate in the thicker part of the soldering layer, resulting in excessively high local temperature of the electronic components, which will cause failure or burning of the electronic components; in the thinner part of the soldering layer, due to the insufficient amount of solder in the soldering layer, the soldering layer is prone to voids, and the soldering layer void rate is high, then the thermal resistance of the solder joint will increase.
[0004] Therefore, reducing the solder void rate of the solder layer and improving the thickness uniformity of the solder layer are crucial to improving the quality of the solder layer and thus ensuring the reliable operation of electronic components during service. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a flat composite solder and a preparation method and application thereof.
[0006] To achieve the above object, the technical solution adopted by the present invention is as follows: In a first aspect, a flat composite solder is provided, wherein the flat solder is provided with a plurality of evenly distributed through holes and metal balls embedded in the through holes;
[0007] The shape of the through hole is at least one of an ellipse and a polygon, and the ratio of the area of the through hole to the large circle area of the metal ball is 2-8; the melting point of the metal ball - the melting point of the solder ≥ 200°C; the diameter of the metal ball is the same as the thickness of the flat solder.
[0008] In some embodiments, the ratio of the area of the through hole to the great circle area of the metal sphere is 4-6.
[0009] In some embodiments, the distance between adjacent through holes is 3-9 mm.
[0010] In some embodiments, the polygon is at least one of a right triangle, an isosceles triangle, a rectangle, a trapezoid, a parallelogram, and a rhombus.
[0011] In some embodiments, the metal is at least one of copper, copper alloy, nickel, nickel alloy, silver, silver alloy, and gold.
[0012] In some embodiments, the flat solder is one of tin-based solder, lead-based solder, bismuth-based solder, indium-based solder, zinc-based solder, antimony-based solder, and aluminum-based solder.
[0013] In some embodiments, the surface of the flat composite solder includes flux.
[0014] In a second aspect, a method for preparing the flat composite solder is provided, comprising the following steps:
[0015] The raw materials of the solder are melted in proportion and cast into an ingot, and then the ingot is rolled to form a flat solder;
[0016] A through hole is punched out on the flat solder, and then a metal ball is embedded in the through hole to obtain a flat composite solder.
[0017] In some embodiments, the method for preparing the flat composite solder further includes coating a flux on the surface of the flat composite solder.
[0018] In a third aspect, a use of the flat composite solder in welding electronic components is provided.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: a plurality of evenly distributed through holes are provided on the flat solder, and metal balls with a melting point 200°C higher than that of the solder are embedded in the through holes, so that the metal balls will not roll, and there will be no loss, dislocation or stacking of the metal balls, thereby improving the uniform distribution of the metal balls in the solder and thus improving the thickness uniformity of the welding layer; on the other hand, there is a gap between the through hole and the metal ball, so that the gas generated during the welding process is discharged from the gap, thereby reducing the welding void rate; on the one hand, during the welding process, the metal ball will not melt, and the wetting effect of the metal ball and the molten solder improves the welding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a structural diagram of the flat composite solder of Example 1;
[0021] Figure 2 This is a structural diagram of the flat composite solder of Example 7;
[0022] Figure 3 This is a structural diagram of the flat composite solder of Example 9. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0024] As used herein:
[0025] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0026] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0027] When amount, concentration or other value or parameter is represented by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1-5", described range should be interpreted as including range "1-4", "1-3", "1-2", "1-2 and 4-5", "1-3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0028] In these examples, parts and percentages are by mass unless otherwise indicated.
[0029] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0030] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0031] In a first aspect, a flat composite solder is provided, wherein the flat solder is provided with a plurality of evenly distributed through holes and metal balls embedded in the through holes;
[0032] The shape of the through hole is at least one of an ellipse and a polygon, and the ratio of the area of the through hole to the large circle area of the metal ball is 2-8; the melting point of the metal ball - the melting point of the solder ≥ 200°C; the diameter of the metal ball is the same as the thickness of the flat solder.
[0033] Specifically, the ratio of the area of the through hole to the great circle area of the metal ball can be but is not limited to 2, 2.2, 2.5, 2.7, 3, 3.3, 3.5, 3.8, 4, 4.2, 4.5, 4.7, 5, 5.3, 5.5, 5.8, 6.2, 6.5, 6.7, 7, 7.3, 7.5, 7.8, 8.
[0034] Specifically, the melting point of the metal ball - the melting point of the solder can be but not limited to 200°C, 220°C, 250°C, 270°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1200°C.
[0035] The present invention provides a plurality of evenly distributed through holes on the flat solder, and embeds metal balls into the through holes, so that the metal balls will not roll, and there will be no loss, dislocation or stacking of the metal balls, thereby improving the uniform distribution of the metal balls in the solder, thereby improving the thickness uniformity of the welding layer.
[0036] When the through hole is elliptical, the diameter of the metal ball is the same as the short axis of the ellipse, that is, the major circle of the metal ball and the short axis of the ellipse are tangent, so that the metal ball can be stably embedded in the through hole; if the through hole is polygonal, the metal ball is tangent to at least two sides of the polygon, so that the metal ball can be stably embedded in the through hole.
[0037] The ratio of the area of the through hole to the large circle area of the metal ball is one of the factors affecting the welding performance of the flat composite solder. The present invention selects a specific ratio of the area of the through hole to the large circle area of the metal ball, which can not only ensure that the metal ball is stably embedded in the through hole and does not fall off, but also that there is a gap between the edge of the through hole and the edge of the metal ball, so that the gas generated during the welding process can be discharged from the gap. In addition, it can also ensure that the molten solder during the welding process is filled and evenly distributed, reducing the welding void rate, improving the uniformity of the welding layer thickness, and improving the welding quality; if the ratio of the area of the through hole to the large circle area of the metal ball is less than 2, the gas generated during the welding process is not easy to be discharged, resulting in a high welding void rate; if the ratio of the area of the through hole to the large circle area of the metal ball is greater than 8, the solder is missing too much, resulting in the molten solder being unable to reflux and fill the gap during the welding process, resulting in an increase in the welding void rate, or even a cold solder. Therefore, the present invention further preferably has a ratio of the area of the through hole to the large circle area of the metal ball of 4-6 to obtain a flat solder with a low welding void rate and uniform welding layer thickness.
[0038] By limiting the difference between the melting point of the metal ball and the melting point of the solder to at least 200°C, it can be ensured that the metal ball will not melt during the welding process, and the welding layer can be prevented from tilting due to the uneven flow of the molten solder, thereby improving the thickness uniformity of the welding layer. If the diameter of the metal ball is smaller than the thickness of the flat solder, when the solder melts, the upper and lower welding surfaces do not contact the metal ball, resulting in uneven flow of the molten solder, and there may be bubbles between the solder and the metal ball, which leads to a decrease in the thickness uniformity of the welding layer, and the void rate of the thinner parts of the welding layer may also increase; if the diameter of the metal ball is larger than the thickness of the flat solder, when the solder melts, the molten solder is suspended, and the upper and lower welding surfaces cannot contact the molten solder, resulting in an increase in the welding void rate, or even a cold solder; in addition, since the diameter of the metal ball is larger than the thickness of the flat solder, the thickness of the molten solder is lower than that of the metal ball, and the distribution uniformity of the solder cannot be controlled by the metal ball, resulting in a decrease in the thickness uniformity of the welding layer.
[0039] In some embodiments, the spacing between adjacent through holes is 3-9 mm; for example, it can be but is not limited to 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, and 8 mm.
[0040] The spacing between adjacent through holes in the present invention refers to the distance between the edges of adjacent through holes. If the spacing between adjacent through holes is less than 3 mm, it will be inconvenient to demold during the processing of the through holes. Moreover, if the through holes are too dense, the strength of the flat solder will decrease, thereby causing the flat solder to deform and even tear the through holes, thereby reducing the yield rate of the flat solder with through holes on the surface. If the spacing between adjacent through holes is greater than 9 mm, the gas generated during the welding process will be difficult to discharge due to the long distance between the through holes, resulting in an increase in the welding void rate.
[0041] In some embodiments, the polygon is at least one of a right triangle, an isosceles triangle, a rectangle, a trapezoid, a parallelogram, and a rhombus.
[0042] Compared with polygonal through holes, on the one hand, elliptical through holes have smooth edges and are easy to demold during through hole processing. The processing is easy and low-cost, which is beneficial to improving the yield rate of flat solder with through holes on the surface. On the other hand, when the metal ball is inscribed in the elliptical through hole, the contact area between the through hole and the metal ball is larger, which can further improve the stability of the metal ball. The preferred shape of the through hole in the present invention is an elliptical shape.
[0043] In some embodiments, the metal is at least one of copper, copper alloy, nickel, nickel alloy, silver, silver alloy, and gold.
[0044] The metal balls composed of the above metals can ensure that the metal balls and molten solder are wetted during the welding process, thereby reducing the welding void rate, improving the uniformity and stability of the welding layer, and improving the welding quality.
[0045] In some embodiments, the flat solder is one of tin-based solder, lead-based solder, bismuth-based solder, indium-based solder, zinc-based solder, antimony-based solder, and aluminum-based solder.
[0046] The flat solder in the present invention can be prepared by a preparation method known in the art, or purchased as a commercial product.
[0047] In some embodiments, the surface of the flat composite solder includes flux.
[0048] In a second aspect, the method for preparing the flat composite solder of the present invention comprises the following steps:
[0049] The raw materials of the solder are melted in proportion and cast into an ingot, and then the ingot is rolled to form a flat solder;
[0050] A through hole is punched out on the flat solder, and then a metal ball is embedded in the through hole to obtain a flat composite solder.
[0051] Those skilled in the art can select different melting temperatures, casting temperatures, calendering processes, etc. according to different raw materials.
[0052] In some embodiments, the method for preparing the flat composite solder further includes coating a flux on the surface of the flat composite solder.
[0053] The surface of the flat composite solder of the present invention is coated with flux, and the flux is used to remove the oxide layer on the solder surface and the welding surface, thereby improving the welding quality. If formic acid or hydrogen is used for reduction welding, the surface of the flat composite solder of the present invention may not be coated with flux, and formic acid or hydrogen is used to remove the oxide layer on the solder surface and the welding surface, thereby improving the welding quality.
[0054] Specifically, the present invention does not impose any specific limitation on the coating method of the soldering flux, as long as the soldering flux can be coated on the surface of the flat composite solder, such as brush coating, dip coating, roller coating, spray coating, etc.
[0055] In a third aspect, a use of the flat composite solder in welding electronic components is provided.
[0056] Example 1
[0057] like Figure 1As shown, this embodiment provides a flat composite solder, on which a plurality of evenly distributed elliptical through holes are provided, the size of the flat solder is 57*48.5*0.3mm, the ratio of the area of the through hole to the great circle area of the metal ball is 5, the short axis of the ellipse is 0.3mm, the diameter of the metal ball is 0.3mm, and the spacing between adjacent through holes is 3mm; the metal ball is a copper ball with a melting point of 1085°C, and the flat solder is Sn95Sb5 with a melting point of 240°C.
[0058] This embodiment also provides a method for preparing a flat composite solder, comprising the following steps:
[0059] A tin ingot and an antimony ingot with a mass ratio of Sn:Sb=95:5 are melted and cast to obtain a Sn95Sb5 ingot, and the Sn95Sb5 ingot is rolled to form a flat solder with a thickness of 0.3 mm;
[0060] Elliptical through holes are punched out on the flat solder. The spacing between adjacent through holes is 3 mm, the minor axis of the ellipse is 0.3 mm, and the ratio of the area of the through hole to the great circle area of the metal ball is 5.
[0061] The metal ball is embedded in the elliptical through hole and punched out to obtain a flat composite solder with a size of 57*48.5*0.3 mm.
[0062] Example 2
[0063] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the ratio of the area of the through hole to the large circle area of the metal ball is 4, and the rest is the same as that of Embodiment 1.
[0064] Example 3
[0065] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the ratio of the area of the through hole to the large circle area of the metal ball is 3, and the rest is the same as that of Embodiment 1.
[0066] Example 4
[0067] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the ratio of the area of the through hole to the large circle area of the metal ball is 6, and the rest is the same as that of Embodiment 1.
[0068] Example 5
[0069] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the ratio of the area of the through hole to the large circle area of the metal ball is 2, and the rest is the same as that of Embodiment 1.
[0070] Example 6
[0071] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the ratio of the area of the through hole to the large circle area of the metal ball is 8, and the rest is the same as that of Embodiment 1.
[0072] Example 7
[0073] like Figure 2 As shown, this embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the shape of the through hole is rectangular, and the rest is the same as that of Embodiment 1.
[0074] Example 8
[0075] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the through hole is in the shape of a right triangle, the two right-angled sides of the right triangle are 1 mm and 0.71 mm respectively, and the rest is the same as that of Embodiment 1.
[0076] Example 9
[0077] like Figure 3 As shown, this embodiment provides a flat composite solder. The only difference between the flat composite solder of this embodiment and that of Embodiment 1 is that the shape of the through hole is an isosceles triangle, the base of the isosceles triangle is 1.04 mm, and the waist is 0.856 mm. The rest is the same as that of Embodiment 1.
[0078] Example 10
[0079] This embodiment provides a flat composite solder. The only difference between the flat composite solder of this embodiment and that of Embodiment 1 is that the shape of the through hole is a right-angled trapezoid, the upper base of the right-angled trapezoid is 0.9 mm, the lower base is 1.455 mm, and the waist is 0.3 mm. The rest is the same as Embodiment 1.
[0080] Embodiment 11
[0081] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the spacing between adjacent through holes is 9 mm, and the rest is the same as that of Embodiment 1.
[0082] Example 12
[0083] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the metal ball is a nickel ball with a melting point of 1445° C., and the rest is the same as that of Embodiment 1.
[0084] Embodiment 13
[0085] This embodiment provides a flat composite solder. The flat composite solder of this embodiment is different from that of Embodiment 1 only in that the metal ball is an Ag72Cu28 ball with a melting point of 779°C, and the rest is the same as that of Embodiment 1.
[0086] Embodiment 14
[0087] This embodiment provides a flat composite solder. The difference between the flat composite solder of this embodiment and that of Embodiment 1 is that a rosin-based flux is coated on the surface of the flat composite solder. The mass of the flux is 0.4% of the mass of the flat composite solder. The rest is the same as that of Embodiment 1.
[0088] Comparative Example 1
[0089] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and that in Example 1 is that the ratio of the area of the through hole to the large circle area of the metal ball is 1.33, and the rest is the same as that in Example 1.
[0090] Comparative Example 2
[0091] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and that in Example 1 is that the ratio of the area of the through hole to the large circle area of the metal ball is 10, and the rest is the same as that in Example 1.
[0092] Comparative Example 3
[0093] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and Example 1 is that the shape of the through hole is a regular hexagon with a side length of 0.173; the ratio of the area of the through hole to the great circle area of the metal ball is 1.1, and the rest is the same as Example 1.
[0094] Comparative Example 4
[0095] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and that in Example 1 is that the through hole is circular in shape with a diameter of 0.3 mm. The rest is the same as in Example 1.
[0096] Comparative Example 5
[0097] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and that in Example 1 is that the spacing between adjacent through holes is 12 mm, and the rest is the same as that in Example 1.
[0098] Comparative Example 6
[0099] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and that in Example 1 is that the metal ball is a lead ball with a melting point of 327° C., and the rest is the same as in Example 1.
[0100] Comparative Example 7
[0101] This comparative example provides a flat composite solder. The only difference between the flat composite solder in this comparative example and that in Example 1 is that no metal ball is embedded in the through hole. The rest is the same as that in Example 1.
[0102] Comparative Example 8
[0103] This comparative example provides a flat composite solder, and a preparation method thereof comprises the following steps:
[0104] Tin ingots and antimony ingots with a mass ratio of Sn:Sb=95:5 are melted and cast into ingots, and then rolled to form flat solder with a thickness of 0.3 mm. The melting point of the flat solder is 240°C.
[0105] Then, copper balls with a diameter of 0.3 mm and a melting point of 1085°C are evenly sprinkled on the surface of the flat solder, and then the copper balls are pressed into the flat solder. After cutting, a flat composite solder with a size of 57*48.5*0.3 mm is obtained.
[0106] Comparative Example 9
[0107] This comparative example provides a flat composite solder, and a preparation method thereof comprises the following steps:
[0108] Mixing and melting a tin ingot and an antimony ingot in a mass ratio of Sn:Sb=95:5 to obtain a molten liquid;
[0109] Then, a copper ball with a diameter of 0.3 mm and a melting point of 1085°C is added to the molten liquid, cooled and solidified into a brazing material block;
[0110] The solder block is rolled and cut to obtain a flat composite solder with a size of 57*48.5*0.3 mm.
[0111] Comparative Example 10
[0112] This comparative example provides a flat composite solder, and a preparation method thereof comprises the following steps:
[0113] The Sn95Sb5 alloy solder powder was mixed with a copper ball with a diameter of 0.3 mm, and then pressed into a flat composite solder with a size of 57*48.5*0.3 mm.
[0114] Comparative Example 11
[0115] This comparative example provides a flat solder, and a preparation method thereof comprises the following steps:
[0116] Tin ingots and antimony ingots with a mass ratio of Sn:Sb=95:5 are melted and cast to obtain Sn95Sb5 ingots. The Sn95Sb5 ingots are rolled and punched to obtain flat solder with a size of 57*48.5*0.3mm. The melting point of the flat solder is 240°C.
[0117] Comparative Example 12
[0118] This comparative example provides a flat solder. The difference between the flat solder in this comparative example and comparative example 11 is that the surface of the flat solder is coated with the same flux as that in Example 11, and the mass of the flux is 0.4% of the mass of the flat solder.
[0119] Performance Testing
[0120] The welding performance of the flat composite solder or flat solder obtained in the above examples and comparative examples was tested.
[0121] The preparation method of the welded parts is as follows:
[0122] Welded material: copper-clad DBC board with a size of 57*48.5*2mm;
[0123] Welding method: Flat composite solder or flat solder without flux on the surface is used as test group 1, and flat composite solder or flat solder coated with flux on the surface is used as test group 2;
[0124] The welding method of test group 1 is: two copper-clad DBC boards are sandwiched between the flat composite solder or flat solder of test group 1, and vacuum formic acid reflow soldering is performed to obtain a welded part;
[0125] The welding method of test group 2 is: the flat composite solder or flat solder of test group 2 is sandwiched between two copper-clad DBC boards, and reflow soldering is performed at normal pressure to obtain a welded part;
[0126] The test method for welding void rate is: use ultrasonic scanner to detect voids in welded parts. The smaller the void rate of welding layer, the better the welding quality.
[0127] The test method for the difference in welding layer thickness is: measure the maximum and minimum thickness of the welded part by a spiral micrometer. The difference in welding layer thickness = maximum thickness - minimum thickness. The greater the difference in welding layer thickness, the more uneven the thickness of the welding layer, that is, the greater the inclination of the welding layer.
[0128] The performance test results are shown in Table 1.
[0129] Table 1 Performance test results
[0130]
[0131]
[0132] It can be seen from the data of test group 1 in Table 1 that for flat solder with no flux on the surface, the welding void rate of the flat composite solder with no flux on the surface of the present invention is 0.02-1.01%, and the welding layer thickness difference is 0.003-0.025mm, and the welding void rate and welding layer thickness difference are significantly improved.
[0133] By comparing Examples 1-6 and Comparative Example 1-2, it can be seen that when the ratio of the area of the through hole to the large circle area of the metal ball is 4-6, the welding void rate of the obtained flat composite solder is 0.02-0.50%, and the welding layer thickness difference is 0.003-0.009mm, indicating that when the ratio of the area of the through hole to the large circle area of the metal ball is 4-6, the welding void rate and welding layer thickness difference of the obtained flat composite solder are lower.
[0134] By comparing Example 1, Examples 7-10 and Comparative Examples 3-4, it can be seen that only when the shape of the through hole is within the protection scope of the present invention, a flat composite solder with a lower welding void rate and welding layer thickness difference can be obtained.
[0135] By comparing Example 1, Example 11 and Comparative Example 5, it can be seen that the spacing between adjacent through holes is 3-9 mm, the welding void rate of the obtained flat solder is 0.02-1.01%, and the welding layer thickness difference is 0.003-0.025 mm, indicating that the spacing between adjacent through holes is 3-9 mm, which can reduce the welding void rate and welding layer thickness difference of the flat composite solder.
[0136] By comparing Example 1, Examples 12-13 and Comparative Example 6, it can be seen that when the melting point of the metal ball minus the melting point of the solder is less than 200° C., the solder void rate and solder layer thickness difference of the obtained flat composite solder are significantly increased.
[0137] Comparing Comparative Example 7 and Comparative Example 11, it can be seen that Comparative Example 7 sets a through hole on the flat solder, which can reduce the welding void rate of the flat composite solder, but because no metal ball is embedded in the through hole, the difference in thickness of the welding layer is basically not improved. Comparing Example 1 and Comparative Example 7, it can be seen that although Comparative Example 7 sets a through hole on the flat solder to reduce the welding void rate, the lack of metal balls embedded in the through hole causes the welding layer to be tilted, and the welding void rate of the thinner part of the welding layer is large, which weakens the effect of the through hole on reducing the welding void rate, resulting in a larger welding void rate than Example 1 as a whole. Comparing Example 1 and Comparative Example 11, it can be seen that setting a through hole on the flat solder and embedding a metal ball in the through hole can significantly reduce the welding void rate and the difference in thickness of the welding layer.
[0138] By comparing Example 1 with Comparative Examples 8-10, it can be seen that in the method of sprinkling metal balls on the surface of the solder and then pressing them into the solder, during the preparation process of the flat composite solder, the metal balls roll, resulting in the loss, dislocation, and stacking of the metal balls, thereby resulting in uneven distribution of the metal balls, which increases the welding void rate and welding layer thickness difference of the flat composite solder; in the method of adding metal balls to the molten solder liquid and then solidifying, since the distribution of the metal balls in the solder molten liquid is random, this method also has the problem of uneven distribution of metal balls, thereby increasing the welding void rate and welding layer thickness difference of the flat composite solder; in the method of mixing solder powder and metal balls and then pressing them into a flat composite solder, on the one hand, the solder components in the flat composite solder prepared by this method are easily oxidized, resulting in a high welding void rate, and on the other hand, the cost of preparing the flat composite solder by this method is high, which is not conducive to industrial production.
[0139] From the data of test group 2 (ie, Example 14 and Comparative Example 12), it can be seen that for the flat solder with flux on the surface, the welding void rate and welding layer thickness difference of the flat composite solder with flux on the surface of the present invention are also significantly improved.
[0140] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A flat composite solder, characterized in that: The flat solder is provided with a plurality of evenly distributed through holes and metal balls embedded in the through holes; The shape of the through hole is at least one of an ellipse and a polygon, and the ratio of the area of the through hole to the large circle area of the metal ball is 2-8; the melting point of the metal ball - the melting point of the solder ≥ 200°C; the diameter of the metal ball is the same as the thickness of the flat solder.
2. The flat composite solder according to claim 1, characterized in that: The ratio of the area of the through hole to the great circle area of the metal ball is 4-6.
3. The flat composite solder according to claim 1, characterized in that: The distance between adjacent through holes is 3-9 mm.
4. The flat composite solder according to claim 1, characterized in that: The polygon is at least one of a right triangle, an isosceles triangle, a rectangle, a trapezoid, a parallelogram, and a rhombus.
5. The flat composite solder according to claim 1, characterized in that: The metal is at least one of copper, copper alloy, nickel, nickel alloy, silver, silver alloy and gold.
6. The flat composite solder according to claim 1, characterized in that: The flat solder is one of tin-based solder, lead-based solder, bismuth-based solder, indium-based solder, zinc-based solder, antimony-based solder, and aluminum-based solder.
7. The flat composite solder according to any one of claims 1 to 6, characterized in that: The surface of the flat composite solder includes flux.
8. A method for preparing the flat composite solder according to any one of claims 1 to 7, characterized in that: The following steps are involved: The raw materials of the solder are melted in proportion and cast into an ingot, and then the ingot is rolled to form a flat solder; A through hole is punched out on the flat solder, and then a metal ball is embedded in the through hole to obtain a flat composite solder.
9. The method for preparing a flat composite solder according to claim 8, characterized in that: The method for preparing the flat composite solder further comprises coating a soldering flux on the surface of the flat composite solder.
10. Use of the flat composite solder according to any one of claims 1 to 7 in welding electronic components.
Citation Information
Patent Citations
Method for producing metal and diamond composite body
CN101480744A
Adapter plate for filling through holes by wafer-level re-balling printing and manufacturing method thereof
CN102683309A
Soldering lug for welding power module
CN105537793A
Composite soldering lug and preparation method thereof
CN116275681A
Ball mounting structure beneficial to welding spot protection and welding
CN220456408U