Surfacing remanufacturing method of high-pressure well head body

By using a pulsed argon arc welding method with a hot wire and remanufacturing with high-nickel alloy materials, the problem of wear on the sealing surface of high-pressure wellheads was solved, achieving functional restoration and cost reduction.

CN118989855APending Publication Date: 2024-11-22SUZHOU WELLHAM SURFACING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411097688.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

High-pressure wellheads in subsea oil and gas production systems often experience sealing or connection failures due to wear on the sealing and connection surfaces, and existing technologies struggle to effectively restore their function.

Method used

The welding remanufacturing process employs a pulsed argon arc welding method with a hot wire, using high-nickel alloy materials with excellent wear and corrosion resistance. It combines strict testing and heat treatment steps, including preheating, surface flaw detection, local heat treatment, and finishing, to ensure welding quality.

Benefits of technology

It effectively restored the sealing and connection functions of the high-pressure wellhead, reduced material costs, and shortened the manufacturing cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989855A_ABST
    Figure CN118989855A_ABST
Patent Text Reader

Abstract

The invention discloses a surfacing remanufacturing method for a high-pressure well head body. The surfacing remanufacturing method comprises the following steps that after preprocessing, thickness and surface flaw detection is conducted on the area, needing surfacing remanufacturing, of the high-pressure well head body; the current polarity and the wiring mode used for surfacing remanufacturing are direct current positive connection; the stepping distance is that 2.8-3.2 mm is increased every 360 degrees, and 40%-50% of lap joint is formed between every two adjacent channels; the shielding gas in the surfacing process is argon; the interlayer or channel temperature in the surfacing process is not higher than 250 DEG C; after surfacing is completed, local stress relief heat treatment is conducted on a surfacing area; and carrying out surface nondestructive inspection and surfacing layer volume defect inspection. The method has the beneficial effects that a pulse argon arc welding automatic welding method with a hot wire is adopted for surfacing remanufacturing, high-nickel alloy with excellent wear resistance and corrosion resistance is adopted as a surfacing material, the overall material cost is reduced, the whole manufacturing period is shortened, and functional recovery of key parts is completed with extremely low material and manufacturing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surfacing welding of a high-pressure wellhead body, and in particular to a surfacing welding remanufacturing method for a high-pressure wellhead body. Background Art

[0002] High-pressure wellheads play an extremely important role in underwater oil and gas production systems and are the most critical pressure-bearing components. The design pressure of underwater oil and gas production systems is generally not less than 10,000 Psi (70 MPa). Accordingly, high-pressure wellheads use high-yield strength carbon steel as the body material, such as carbon steel materials that meet AISI8630 standards and are 80 Ksi in grade. During long-term actual downhole operations, the sealing surface and connection surface of the wellhead body will experience varying degrees of axial strain or wear, resulting in sealing or connection failure. Summary of the invention

[0003] The object of the present invention is to provide a surfacing welding remanufacturing method for a high-pressure wellhead body to solve the problems raised in the above-mentioned background technology.

[0004] To achieve the above object, the present invention provides the following technical solution: a surfacing welding remanufacturing method for a high-pressure wellhead body, comprising the following steps:

[0005] Step 1: After pre-processing, the appearance inspection and dimensional inspection of the area of ​​the high-pressure wellhead body that needs to be remanufactured by surfacing welding are carried out, and the original damaged area needs to be completely removed;

[0006] Step 2: Perform surface flaw detection on the area of ​​the high-pressure wellhead body that needs surfacing welding and remanufacturing. The preheating temperature before surfacing welding and remanufacturing shall not be less than 150°C;

[0007] Step 3: The current polarity and wiring method used in cladding remanufacturing are direct current positive connection, the workpiece is connected to the positive pole, and the tungsten electrode is connected to the negative pole;

[0008] Step 4: The stepping distance is 2.8-3.2mm for every 360°, and the overlap between the tracks is 40%-50%;

[0009] Step 5: During the cladding process, the protective gas is argon with a purity of not less than 99.999%, and the gas flow rate is 15-17L / min;

[0010] Step 6: The temperature between layers or passes during the cladding process shall not exceed 250°C;

[0011] Step 7: After the cladding is completed, the cladding area is subjected to surface non-destructive testing and cladding layer volume defect testing. The surface non-destructive testing adopts the coloring test (PT) method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified. The cladding layer volume defect inspection adopts the ultrasonic flaw detection (UT) method. The comparison test block adopts a φ1.6mm flat bottom hole. If there is no defect exceeding the standard, it is qualified.

[0012] Step 8: Perform local heat treatment on the surfacing area to eliminate welding stress; attach the crawler electric heating plate to the surface of the surfacing layer and use steel wire to tie it in the longitudinal direction. The crawler electric heating plate should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm; the outer surface of the workpiece corresponding to the surfacing area is insulated with aluminum silicate fiber felt, the insulation thickness is about 100mm, and the width should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm; use K-type thermocouples for temperature measurement, one is placed on the surface of the surfacing layer, and the other is placed on the outer surface of the workpiece;

[0013] Step 9: After the local heat treatment is completed, the surfacing area is subjected to surface non-destructive testing. The surface non-destructive testing adopts the coloring test method. The inspection area should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified;

[0014] Step 10: Finish the surfacing area;

[0015] Step 11: After finishing, the cladding area is subjected to surface non-destructive testing and dimensional inspection. The surface non-destructive testing adopts the coloring inspection method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified;

[0016] Step 12: Finally, perform a pressure test according to the corresponding pressure level, and then perform phosphating treatment on the outer surface.

[0017] For further optimization, in step 1, pre-processing is required to completely remove the original damaged area.

[0018] Further optimized, in the step 2, the product is inspected and accepted without any defects, and then oil and moisture are removed to avoid affecting the quality of the cladding layer, and the preheating temperature before cladding remanufacturing is not less than 150°C.

[0019] Further optimized, in step three, the system pulse frequency is 2.5 Hz and the pulse time is set at 200 milliseconds.

[0020] Further optimized, in step 3, the peak welding current needs to be set at 190-225A, the base current needs to be set at 100-120A, and the welding voltage needs to be set at 10-12V. The hot wire current is set at 20-31A, and the hot wire voltage is 9.9V. The welding speed needs to be set at 26-30cm / min. The wire diameter is 1.2mm or 1.14mm, and the wire feeding speed needs to be set at 130-200cm / min.

[0021] Further optimized, in step 4, the tungsten electrode does not swing during the surfacing process, the diameter of the tungsten electrode is 3.2 mm, and the extended length of the tungsten electrode is 10 to 12 mm.

[0022] Further optimized, in step five, the argon gas with a purity of not less than 99.999% is used, and the gas flow rate is 15 to 17 L / min.

[0023] Further optimized, in step six, the temperature control method of the interlayer temperature is to use a contact thermometer to measure the temperature, and perform local stress relief heat treatment after surfacing.

[0024] Further optimized, in the step seven, the surface nondestructive testing of the weld overlay area and the volume defect testing of the weld overlay layer are carried out. The surface nondestructive testing adopts the coloring test (PT) method. The inspection area should cover the entire weld overlay area and the area of ​​the parent material on both sides of not less than 13mm. The surface is qualified if there are no defects. The volume defect inspection of the weld overlay layer adopts the ultrasonic testing (UT) method. The comparison test block adopts a φ1.6mm flat-bottom hole. It is qualified if there are no defects exceeding the standard.

[0025] Further optimized, in step eight, the local heat treatment equipment includes a temperature measuring thermocouple, a time-temperature recorder and a controller, and the local heat treatment process steps are as follows: after heating to 300°C, the average heating rate of the heating zone should be in the range of 55-150°C / h, heating to the heat treatment temperature of 650°C±10°C, keeping warm for 4-5 hours, and then cooling. Before cooling to 300°C, the average cooling rate of the heating zone should be in the range of 55-150°C / h. After cooling to 300°C, the electric heating plate and the insulation material can be removed, and the workpiece is cooled to room temperature in still air. In step eleven, the outer surface of the workpiece corresponding to the surfacing area is insulated with aluminum silicate fiber felt, the insulation thickness is about 100mm, and the width should cover the entire surfacing area and the area of ​​the parent material on both sides of not less than 13mm. K-type thermocouples are used for temperature measurement, one is placed on the surface of the surfacing layer, and the other is placed on the outer surface of the workpiece.

[0026] Beneficial Effects

[0027] The surfacing welding remanufacturing method of the high-pressure wellhead body provided by the present invention adopts a pulsed argon arc welding automatic welding method with a hot wire, and the surfacing material adopts a high-nickel alloy with excellent wear resistance and corrosion resistance, which reduces the overall material cost and shortens the entire manufacturing cycle, and completes the functional restoration of key components at extremely low material and manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the manufacturing process of the present invention;

[0029] Figure 2 This is a schematic diagram of the pre-processing of the high-pressure wellhead head of the present invention;

[0030] Figure 3 A schematic diagram of a high-pressure wellhead welding location of the present invention;

[0031] Figure 4 It is a schematic diagram of the structure of the high-pressure wellhead body of the present invention. DETAILED DESCRIPTION

[0032] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0033] Example

[0034] like Figure 1-4 As shown, a surfacing welding remanufacturing method for a high-pressure wellhead body comprises the following steps:

[0035] Step 1: After pre-processing, the appearance inspection and dimensional inspection of the area of ​​the high-pressure wellhead body that needs to be remanufactured by surfacing welding are carried out, and the original damaged area needs to be completely removed;

[0036] Step 2: Perform surface flaw detection on the area of ​​the high-pressure wellhead body that needs surfacing welding and remanufacturing. The preheating temperature before surfacing welding and remanufacturing shall not be less than 150°C;

[0037] Step 3: The current polarity and wiring method used in cladding remanufacturing are direct current positive connection, the workpiece is connected to the positive pole, and the tungsten electrode is connected to the negative pole;

[0038] Step 4: The stepping distance is 2.8-3.2mm for every 360°, and the overlap between the tracks is 40%-50%;

[0039] Step 5: During the cladding process, the protective gas is argon with a purity of not less than 99.999%, and the gas flow rate is 15-17L / min;

[0040] Step 6: The temperature between layers or passes during the cladding process shall not exceed 250°C;

[0041] Step 7: After the cladding is completed, the cladding area is subjected to surface non-destructive testing and cladding layer volume defect testing. The surface non-destructive testing adopts the coloring test (PT) method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified. The cladding layer volume defect inspection adopts the ultrasonic flaw detection (UT) method. The comparison test block adopts a φ1.6mm flat bottom hole. If there is no defect exceeding the standard, it is qualified.

[0042] Step 8: Perform local heat treatment on the surfacing area to eliminate welding stress; attach the crawler electric heating plate to the surface of the surfacing layer and use steel wire to tie it in the longitudinal direction. The crawler electric heating plate should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm; the outer surface of the workpiece corresponding to the surfacing area is insulated with aluminum silicate fiber felt, the insulation thickness is about 100mm, and the width should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm; use K-type thermocouples for temperature measurement, one is placed on the surface of the surfacing layer, and the other is placed on the outer surface of the workpiece;

[0043] Step 9: After the local heat treatment is completed, the surfacing area is subjected to surface non-destructive testing. The surface non-destructive testing adopts the coloring test method. The inspection area should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified.

[0044] Step 10: Finish the surfacing area;

[0045] Step 11: After finishing, the cladding area is subjected to surface non-destructive testing and dimensional inspection. The surface non-destructive testing adopts the coloring inspection method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified.

[0046] Step 12: Finally, perform a pressure test according to the corresponding pressure level, and then perform phosphating treatment on the outer surface.

[0047] In this embodiment, in the step one, appearance inspection and dimensional inspection are required to completely remove the original damaged area; in the step two, the product is inspected and accepted without any defects, and then oil and moisture are removed to avoid affecting the quality of the surfacing layer. The preheating temperature before surfacing remanufacturing is not less than 150°C.

[0048] In step 3, the system pulse frequency is 2.5Hz, and the pulse time is set at 200 milliseconds; in step 3, the welding peak current needs to be set at 190-225A, the base current needs to be set at 100-120A, and the welding voltage needs to be set at 10-12V. The hot wire current is set at 20-31A, and the hot wire voltage is 9.9V. The welding speed needs to be set at 26-30cm / min. The wire diameter is 1.2mm or 1.14mm, and the wire feeding speed needs to be set at 130-200cm / min.

[0049] In the step 4, the tungsten electrode does not swing during the surfacing process, the diameter of the tungsten electrode is 3.2 mm, and the extended length of the tungsten electrode is 10 to 12 mm.

[0050] In the step 5, the protective gas during the cladding process is argon gas with a purity of not less than 99.999%, and the gas flow rate is 15 to 17 L / min.

[0051] In the step six, the interlayer temperature is controlled by measuring the temperature using a contact thermometer, and a local stress relief heat treatment is performed after surfacing.

[0052] In the step seven, after the cladding is completed, the cladding area is subjected to surface nondestructive testing and volume defect testing of the cladding layer. The surface nondestructive testing adopts the coloring test (PT) method. The inspection area should cover the entire cladding area and an area of ​​not less than 13 mm of the parent material on both sides. The surface is qualified if there are no defects. The volume defect inspection of the cladding layer adopts the ultrasonic testing (UT) method. The comparison test block adopts a φ1.6mm flat-bottom hole. It is qualified if there are no defects exceeding the standard.

[0053] In the step eight, the local heat treatment equipment includes a temperature measuring thermocouple, a time-temperature recorder and a controller. The local heat treatment process steps are as follows: after heating to 300°C, the average heating rate of the heating zone should be in the range of 55-150°C / h, heating to the heat treatment temperature of 650°C±10°C, keeping warm for 4-5 hours, and then cooling. Before cooling to 300°C, the average cooling rate of the heating zone should be in the range of 55-150°C / h. After cooling to 300°C, the electric heating plate and the insulation material can be removed, and the workpiece is cooled to room temperature in still air. In the step eleven, the outer surface of the workpiece corresponding to the surfacing area is insulated with aluminum silicate fiber felt, the insulation thickness is about 100mm, and the width should cover the entire surfacing area and the area of ​​the parent material on both sides of not less than 13mm. K-type thermocouples are used for temperature measurement, one is placed on the surface of the surfacing layer, and the other is placed on the outer surface of the workpiece.

[0054] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the invention content within the protection scope of the present invention.

Claims

1. A surfacing welding remanufacturing method for a high-pressure wellhead body, characterized in that: The following steps are involved: Step 1: After pre-processing, the appearance inspection and dimensional inspection of the area of ​​the high-pressure wellhead body that needs to be remanufactured by surfacing welding are carried out, and the original damaged area needs to be completely removed; Step 2: Perform surface flaw detection on the area of ​​the high-pressure wellhead body that needs surfacing welding and remanufacturing. The preheating temperature before surfacing welding and remanufacturing shall not be less than 150°C; Step 3: The current polarity and wiring method used in cladding remanufacturing are direct current positive connection, the workpiece is connected to the positive pole, and the tungsten electrode is connected to the negative pole; Step 4: The stepping distance is 2.8-3.2mm for every 360°, and the overlap between the tracks is 40%-50%; Step 5: During the cladding process, the protective gas is argon with a purity of not less than 99.999%, and the gas flow rate is 15-17L / min; Step 6: The temperature between layers or passes during the cladding process shall not exceed 250°C; Step 7: After the cladding is completed, the cladding area is subjected to surface non-destructive testing and cladding layer volume defect testing. The surface non-destructive testing adopts the coloring test (PT) method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified. The cladding layer volume defect inspection adopts the ultrasonic flaw detection (UT) method. The comparison test block adopts a φ1.6mm flat bottom hole. If there is no defect exceeding the standard, it is qualified. Step 8: Perform local heat treatment on the surfacing area to eliminate welding stress; attach the crawler electric heating plate to the surface of the surfacing layer and use steel wire to tie it in the longitudinal direction. The crawler electric heating plate should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm; the outer surface of the workpiece corresponding to the surfacing area is insulated with aluminum silicate fiber felt, the insulation thickness is about 100mm, and the width should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm; use K-type thermocouples for temperature measurement, one is placed on the surface of the surfacing layer, and the other is placed on the outer surface of the workpiece; Step 9: After the local heat treatment is completed, the surfacing area is subjected to surface non-destructive testing. The surface non-destructive testing adopts the coloring test method. The inspection area should cover the entire surfacing area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified. Step 10: Finish the surfacing area; Step 11: After finishing, the cladding area is subjected to surface non-destructive testing and dimensional inspection. The surface non-destructive testing adopts the coloring inspection method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. If there is no defect on the surface, it is qualified. Step 12: Finally, perform a pressure test according to the corresponding pressure level, and then perform phosphating treatment on the outer surface.

2. The surfacing welding remanufacturing method of the high-pressure wellhead body according to claim 1 is characterized in that: In step 1, the original damaged area needs to be completely removed.

3. The surfacing welding remanufacturing method of the high-pressure wellhead body according to claim 1 is characterized in that: In the step 2, the product is inspected and accepted without any defects, and then oil and water are removed to avoid affecting the quality of the cladding layer. The preheating temperature before cladding remanufacturing is not less than 150°C.

4. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In step three, the system pulse frequency is 2.5 Hz, and the pulse time is set at 200 milliseconds.

5. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In step 3, the peak welding current needs to be set at 190-225A, the base current needs to be set at 100-120A, and the welding voltage needs to be set at 10-12V. The hot wire current of the welding wire is set at 20-31A, and the hot wire voltage is 9.9V. The welding speed needs to be set at 26-30cm / min. The diameter of the welding wire is 1.2mm or 1.14mm, and the wire feeding speed needs to be set at 130-200cm / min.

6. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In the step 4, the tungsten electrode does not swing during the surfacing process, the diameter of the tungsten electrode is 3.2 mm, and the extended length of the tungsten electrode is 10 to 12 mm.

7. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In the step 5, the protective gas is argon gas with a purity of not less than 99.999%, which meets the requirements of AWS A5.32-I1 standard, and the protective gas flow rate is 15-17 L / min.

8. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In the step six, the interlayer temperature is controlled by measuring the temperature using a contact thermometer, and a local stress relief heat treatment is performed after surfacing.

9. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In the step seven, the surface nondestructive testing of the cladding area and the volume defect inspection of the cladding layer are carried out. The surface nondestructive testing adopts the coloring test (PT) method. The inspection area should cover the entire cladding area and the area of ​​the parent material on both sides that is not less than 13mm. The surface is qualified if there are no defects. The volume defect inspection of the cladding layer adopts the ultrasonic testing (UT) method. The comparison test block adopts a φ1.6mm flat-bottom hole. It is qualified if there are no defects exceeding the standard.

10. The surfacing welding remanufacturing method of a high-pressure wellhead body according to claim 1, characterized in that: In the step eight, the local heat treatment equipment includes a temperature measuring thermocouple, a time-temperature recorder and a controller. The local heat treatment process steps are as follows: after heating to 300°C, the average heating rate of the heating zone should be in the range of 55-150°C / h, heating to the heat treatment temperature of 650°C±10°C, keeping warm for 4-5 hours, and then cooling. Before cooling to 300°C, the average cooling rate of the heating zone should be in the range of 55-150°C / h. After cooling to 300°C, the electric heating plate and the insulation material can be removed, and the workpiece is cooled to room temperature in still air. In the step eleven, the outer surface of the workpiece corresponding to the surfacing area is insulated with aluminum silicate fiber felt, the insulation thickness is about 100mm, and the width should cover the entire surfacing area and the area of ​​the parent material on both sides of not less than 13mm. K-type thermocouples are used for temperature measurement, one is placed on the surface of the surfacing layer, and the other is placed on the outer surface of the workpiece.