Plunger machining method
Through plunger processing methods, including heat treatment, nitriding treatment and DLC coating formation, the problem of insufficient performance of plunger materials in the prior art is solved, significantly improve the performance and service life of the plunger, and enhance the fuel injection system Reliability and oil supply uniformity.
Patent Information
- Application Number
- CN202411210900.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to significantly improve the performance and service life of the plunger, especially in fuel injection systems with high precision and high strength requirements. The material performance and processing technology of the plunger are insufficient, which affects the fuel supply uniformity of the fuel engine and reliability.
The plunger processing method is adopted, including heating, insulation, quenching, deep cooling treatment, tempering, nitriding and plasma-enhanced chemical vapor deposition to form a DLC coating to form a relatively gentle hardness gradient, and improve the comprehensive mechanical properties and surface hardness of the material. , and enhance the self-lubricating effect.
It significantly improves the performance and service life of the plunger. By improving the strength and toughness of the material, the hardness of the nitride layer and the DLC coating are enhanced, the plunger strengthening and self-lubricating effect is achieved, and the reliability of the fuel injection system is improved. and oil supply uniformity.
Smart Images

Figure CN118989875A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the processing of marine engine parts, and in particular to a plunger processing method. Background Art
[0002] The plunger pair is one of the key components of the fuel injection system of the fuel engine. It is a precision pair consisting of a plunger and a plunger sleeve. Its working principle is: the reciprocating motion of the plunger in the plunger sleeve forms the function of the fuel injection pump to suck and pump oil; its basic functions are: pressurizing the fuel, controlling the fuel supply time and fuel supply metering. It has high requirements for technical indicators and precision indicators, special product structure, and product quality has a great impact on the fuel supply uniformity of the fuel injection system, the allowable pump end injection pressure, the reliability of the system, and the fuel working process and performance indicators of the fuel engine, which directly affects the normal operation and reliability of the fuel engine. Summary of the invention
[0003] The purpose of the present invention is to provide a plunger processing method, which can significantly improve the performance and service life of the plunger.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A plunger processing method comprises the following steps: S1, heating, heat preservation, quenching, deep cryogenic treatment and tempering are performed on the rough-machined plunger workpiece in sequence; S2, semi-finishing the plunger workpiece after tempering; S3, nitriding treatment, forming a nitrided layer on the surface of the plunger workpiece at a preset position; S4, forming a DLC coating on the nitride layer.
[0005] Furthermore, the heating and heat preservation in S1 includes: firstly heating the rough-machined plunger workpiece to 850±10°C and keeping it warm for 20-30 minutes, then heating it to 900±10°C and keeping it warm for 60-90 minutes, and finally heating it to 1180±10°C and keeping it warm for 20-25 minutes.
[0006] Furthermore, the quenching in S1 is vacuum quenching, water quenching or oil quenching.
[0007] Furthermore, the quenching in S1 is vacuum gas quenching, which specifically includes: placing the roughly machined plunger workpiece in a heating furnace, drawing a vacuum, and then heating and keeping it warm. After the insulation is completed, quenching is performed using 2-5 bar nitrogen, and quenching is performed to 60° C. or below before taking it out of the furnace.
[0008] Furthermore, the tempering times in S1 are at least three times, the tempering temperature is 560±10° C., and the tempering time is 120-150 min.
[0009] Furthermore, the nitriding treatment in S3 includes: placing the semi-finished plunger workpiece as a cathode in a nitriding furnace containing a nitrogen medium, then raising the temperature in the nitriding furnace to 560±10°C and keeping it warm, while introducing the nitrogen-containing medium at a rate of 0.7~1L / min, maintaining the furnace pressure at 300±20Pa, and keeping it warm for 1500~1800min; after the nitriding is completed, nitrogen is introduced to maintain positive pressure, the furnace is cooled to 100°C or below, and the furnace is air-cooled to room temperature.
[0010] Furthermore, a DLC coating is formed on the nitride layer by using a plasma enhanced chemical vapor deposition method.
[0011] Furthermore, before performing S4, the plunger workpiece after the nitriding treatment is finely ground, cleaned, and etched.
[0012] Furthermore, after the DLC coating is formed, the plunger workpiece is polished.
[0013] Furthermore, the material grade of the plunger workpiece in S1 is W6Mo5Cr4V2.
[0014] Beneficial effects of the present invention: The present invention first performs heat treatment on the rough-machined plunger workpiece to improve the comprehensive mechanical properties of the material, so that the material has higher strength and toughness, which is convenient for subsequent processing. Then, a nitriding layer is formed on the surface of the preset position of the plunger workpiece through nitriding treatment; finally, a DLC coating is formed on the nitriding layer. Then, the hardness of the plunger workpiece substrate, the nitriding layer located on the surface of the substrate, and the DLC coating located on the surface of the nitriding layer gradually increases, forming a relatively gentle hardness gradient, thereby strengthening the plunger workpiece. In addition, the surface DLC coating not only has a high hardness, but also has a self-lubricating effect, which will significantly improve the performance and service life of the plunger. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 A schematic flow chart of a plunger processing method according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0016] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0017] In one embodiment, see Figure 1 As shown, the present invention provides a plunger processing method, which comprises the following steps: S1, heating, heat preservation, quenching, deep cryogenic treatment and tempering are performed on the rough-machined plunger workpiece in sequence; S2, semi-finishing the plunger workpiece after tempering; S3, nitriding treatment, forming a nitrided layer on the surface of the plunger workpiece at a preset position; S4, forming a DLC coating on the nitride layer.
[0018] The present invention adopts the above method, that is, first heat-treating the rough-machined plunger workpiece to improve the comprehensive mechanical properties of the material, so that the material has high strength and toughness, which is convenient for subsequent processing. Then, a nitriding layer is formed on the surface of the preset position of the plunger workpiece through nitriding treatment; finally, a DLC coating is formed on the nitriding layer. Then, the hardness of the plunger workpiece substrate, the nitriding layer located on the surface of the substrate, and the DLC coating located on the surface of the nitriding layer gradually increases, forming a relatively gentle hardness gradient, which not only ensures the bonding force between the strengthening layer (nitriding layer and DLC coating) and the substrate, but also realizes the strengthening of the plunger workpiece, and improves the core layer hardness and surface hardness of the plunger workpiece. In addition, the surface DLC coating not only has high hardness, but also has a self-lubricating effect, which will significantly improve the performance and service life of the plunger.
[0019] In a preferred embodiment, the heating and heat preservation in S1 includes: first heating the rough-machined plunger workpiece to 850±10℃ and keeping it warm for 20-30min, then heating it to 900±10℃ and keeping it warm for 60-90min, and finally heating it to 1180±10℃ and keeping it warm for 20-25min.
[0020] Specifically, the initial heating and insulation are carried out first, that is, the rough-machined plunger workpiece is placed in the heating furnace, and the heating rate is controlled to avoid uneven temperature caused by too fast or too slow. The target temperature of the initial heating is 850±10℃. This temperature range is to preheat the workpiece so that its internal temperature gradually increases and reduce the impact of subsequent rapid temperature changes on the material. The insulation time of the initial heating is 20~30 minutes to ensure that the internal temperature of the workpiece Then the secondary heating and insulation are carried out. Compared with the initial heating, the target temperature of the secondary heating (900±10℃) is higher, aiming to further soften the material and prepare for the subsequent quenching process. The insulation time of the secondary heating is 60~90 minutes. This longer insulation time is to ensure that the temperature inside the workpiece reaches a completely uniform temperature and the material structure undergoes sufficient transformation to adapt to the subsequent quenching process.
[0021] Finally, the final heating and insulation are carried out. The target temperature of the final heating is 1180±10℃, which is the final heating temperature before quenching, usually called austenitizing temperature. It makes the material completely transformed into austenite structure, preparing for rapid cooling during quenching. The insulation time of the final heating is 20~25 minutes to ensure the complete formation and uniform distribution of austenite structure, and eliminate the residual processing stress inside the material.
[0022] After completing the above heating and insulation processes, the workpiece will undergo quenching, cryogenic treatment and tempering to further improve the performance of the material.
[0023] It should be noted that these heating and holding parameters (such as temperature and time) may vary depending on the specific material type, composition, required performance, and processing equipment. Therefore, in actual operation, they should be optimized and adjusted according to specific circumstances.
[0024] In a preferred embodiment, the quenching in S1 is vacuum gas quenching, water quenching or oil quenching, and specifically, a reasonable selection is made according to the material and performance requirements of the plunger workpiece.
[0025] Furthermore, in order to better meet the application requirements of the plunger workpiece, the quenching in S1 is vacuum gas quenching. Compared with water quenching and oil quenching, vacuum gas quenching can effectively avoid chemical reaction between the material and the medium during the quenching process, reducing surface contamination and oxidation. The vacuum environment is conducive to the discharge of gas inside the material, reducing porosity and defects. In addition, the quenching cooling speed of vacuum gas quenching is relatively fast, which is suitable for materials requiring high hardness and wear resistance.
[0026] The vacuum gas quenching specifically includes: placing the roughly processed plunger workpiece in a heating furnace, drawing a vacuum, and then heating and keeping warm. After the insulation is completed, gas quenching is performed using 2-5 bar nitrogen, and the workpiece is quenched to 60° C. or below before being taken out of the furnace.
[0027] In a preferred embodiment, the tempering times in S1 are at least three times, the tempering temperature is 560±10° C., and the tempering time is 120-150 min.
[0028] The purpose of selecting at least three temperings is to better control the performance changes of the material. Each tempering will affect the hardness, toughness, strength and other properties of the material to a certain extent. Through multiple temperings, these properties can be gradually adjusted and optimized to reach the best state. In addition, multiple temperings can also help to further eliminate internal stress and structural defects, and improve the stability and reliability of the material.
[0029] Tempering temperature: Setting the tempering temperature to 560±10℃ is a choice based on material characteristics and performance requirements. This temperature range can significantly improve the toughness and fatigue resistance of the material while maintaining a certain hardness. If the tempering temperature is too low, it may not be able to fully eliminate internal stress and brittleness; if the temperature is too high, it may cause the material to soften excessively, reducing its hardness and strength.
[0030] Tempering time: The tempering time is controlled within 120-150 minutes each time to ensure that the material can fully undergo structural transformation and stress release during the tempering process. If the tempering time is too short, the expected effect may not be achieved; if the tempering time is too long, the material may be over-softened or have other adverse effects. Therefore, it is necessary to determine the appropriate tempering time based on the type, size and performance requirements of the material.
[0031] It should be noted that when tempering is performed multiple times, the interval time between each tempering and the cooling method should be ensured to meet the process requirements to avoid adverse effects on material properties. The furnace temperature and time should be strictly controlled during the tempering process to ensure that the material is tempered at a uniform temperature. After tempering, the material should be tested and analyzed as necessary to verify whether its performance meets the requirements.
[0032] In a preferred embodiment, the nitriding treatment in S3 specifically includes the following steps: S31, preparation stage: Use the semi-finished plunger workpiece as the cathode, carefully clean and remove the oil, oxides and other impurities on the surface to ensure the quality of the nitriding layer.
[0033] The workpiece is placed in a nitriding furnace, which should be filled with a nitrogen-containing medium, which is usually ammonia or other nitrogen-containing compounds.
[0034] S32, Heating and Insulation: Raise the temperature in the nitriding furnace to 560±10℃ and maintain this temperature for insulation. This temperature is one of the typical temperature ranges for nitriding treatment, which is conducive to the occurrence of nitriding reaction and the formation of nitriding layer. During the heating process, the heating rate should be controlled to avoid deformation or cracking of the workpiece.
[0035] Introducing nitrogen-containing medium: During the heating and insulation process, continuously introduce nitrogen-containing medium (such as ammonia) at a rate of 0.7~1L / min. This rate should be kept stable to ensure the uniformity and controllability of the nitriding process. The nitrogen-containing medium reacts chemically with the surface of the workpiece in the furnace to form a nitriding layer. The thickness and performance of the nitriding layer depend on factors such as nitriding temperature, time, medium flow rate and furnace pressure.
[0036] During the nitriding process, the furnace pressure should be maintained at 300±20Pa. Appropriate furnace pressure is conducive to the nitriding reaction and the control of the quality of the nitriding layer. If the furnace pressure is too high or too low, it may have an adverse effect on the nitriding effect.
[0037] Insulation time: The insulation time of nitriding treatment is usually 1500~1800 minutes, and the specific time depends on the type of material, the required nitriding layer thickness and performance requirements. The longer the insulation time, the thicker the nitriding layer, but too long insulation time may also increase the surface roughness of the workpiece or produce other undesirable phenomena.
[0038] S33, end of nitriding and cooling: When the nitriding time reaches a predetermined value, the introduction of the nitrogen-containing medium is stopped, and nitrogen is continuously introduced to maintain a positive pressure in the furnace, which helps prevent the nitriding layer from being oxidized or contaminated during the cooling process.
[0039] Then, let the furnace cool naturally to 100°C or below. During this process, avoid sharp temperature changes to prevent deformation of the workpiece or cracking of the nitride layer.
[0040] Finally, the workpiece is taken out of the nitriding furnace and air-cooled to room temperature. During the air-cooling process, care should be taken to avoid contact between the workpiece and other hard objects to prevent scratching the nitriding layer.
[0041] It should be noted that during the nitriding process, the changes in parameters such as furnace temperature, pressure, medium flow rate, etc. should be closely monitored and adjusted in time to ensure the nitriding effect. After nitriding, the workpiece should be subjected to necessary testing and analysis to verify whether the quality and performance of the nitriding layer meet the requirements. The nitriding equipment and operating environment should maintain good cleanliness and stability to avoid adverse effects on the nitriding effect.
[0042] In a preferred embodiment, a DLC coating is formed on the nitride layer by plasma enhanced chemical vapor deposition.
[0043] Plasma enhanced chemical vapor deposition (PECVD) is a chemical vapor deposition technology performed at low pressure that enhances the deposition process by introducing plasma in the gas phase, thereby improving the quality and performance of the film. This method can achieve high-quality film growth at relatively low temperatures, and has good control over the film process and high deposition rate.
[0044] The DLC coating prepared by PECVD technology has the characteristics of excellent wear resistance, low friction coefficient, excellent chemical stability and biocompatibility, and is widely used in semiconductor, optics, biomedicine and tribology. By optimizing the process parameters and deposition conditions, DLC coatings with specific properties can be obtained to meet different application requirements.
[0045] In a preferred embodiment, before performing S4, the plunger workpiece after the nitriding treatment is finely ground, cleaned, and etched.
[0046] The main purpose of fine grinding is to further remove the rough part of the nitride layer surface and improve the surface finish and precision of the workpiece. Fine grinding can be done by mechanical grinding or super finishing. Among them, mechanical grinding: using high-precision grinding wheels, sandpaper or wire brushes and other tools for grinding, can remove the tiny bumps and uneven parts on the surface of the nitride layer, making the surface smoother. Super finishing: For extremely high surface quality requirements, super finishing technology can be used, such as magnetic grinding and polishing, ultrasonic mechanical grinding, etc., which can further refine the surface roughness to the nanometer level.
[0047] During fine grinding, it is important to control the grinding force and angle to avoid excessive grinding that may damage the nitride layer or deform the workpiece. After grinding, the workpiece surface should be cleaned in time to remove the debris and residues generated by grinding.
[0048] The purpose of cleaning is to remove oil, dust and other impurities generated during the fine grinding process, as well as oxides and corrosion products on the surface of the nitride layer to ensure the cleanliness and quality of the workpiece surface.
[0049] Specific cleaning methods include: Soaking cleaning: Soak the workpiece in hot water or a specific cleaning solution for a period of time, using heat energy and the action of the cleaning agent to remove surface stains. This method is suitable for large or difficult-to-clean workpieces.
[0050] High-pressure water washing: Use high-pressure water to wash the surface of the workpiece to remove surface attachments and debris. This method is highly efficient, but it is necessary to pay attention to the control of water pressure and washing angle to avoid damage to the workpiece.
[0051] Chemical cleaning: Use dilute acid or alkaline solution to chemically clean the workpiece surface to remove oxides and corrosive substances. This method is effective, but attention should be paid to the concentration of the cleaning solution and the cleaning time to avoid corrosion or damage to the nitride layer.
[0052] During the cleaning process, pay attention to protecting the surface of the workpiece to avoid scratches or collisions. After cleaning, the workpiece should be dried in time to avoid rust caused by residual moisture.
[0053] The purpose of etching is to adjust the surface roughness of the nitride layer to improve the bonding force between the nitride layer and the DLC coating.
[0054] In a preferred embodiment, after the DLC coating is formed, the plunger workpiece is polished. The polishing process can remove tiny defects, scratches and uneven parts on the coating surface, making the surface smoother and more uniform, thereby improving the wear resistance of the workpiece.
[0055] In a preferred embodiment, the material grade of the plunger workpiece in S1 is W6Mo5Cr4V2.
[0056] W6Mo5Cr4V2 is a high speed steel, also known as M2 steel, with high hardness, high wear resistance, high strength and good heat resistance. Its main chemical composition includes carbon, tungsten, molybdenum, chromium and vanadium, which together give W6Mo5Cr4V2 excellent physical and chemical properties.
[0057] In terms of weight percentage, the W6Mo5Cr4V2 includes the following components: 5.50-6.75% of tungsten W, 4.50-5.50% of molybdenum Mo, 3.80-4.40% of chromium Cr, 1.75-2.20% of vanadium V, 0.80-0.90% of carbon C, 0.15-0.40% of manganese Mn, and the balance is Fe and inevitable impurities.
[0058] The following is an explanation with reference to specific examples.
[0059] Embodiment 1, a plunger processing method, comprising the following steps: S1, the rough-machined plunger workpiece is heated, kept warm, quenched, cryogenically treated, and tempered in sequence.
[0060] After rough machining, the plunger workpiece with material grade W6Mo5Cr4V2 is placed in a vacuum gas quenching furnace for gas quenching. First, vacuum is drawn, then the temperature is raised to 850℃ and kept for 25 minutes, then raised to 900℃ and kept for 70 minutes, and finally raised to 1180℃ and kept for 22 minutes. Then, it is quenched with 2bar nitrogen and cooled to below 60℃ before being taken out of the furnace.
[0061] The plunger workpiece is transferred to the ultra-low temperature cold treatment machine within half an hour after being taken out of the furnace, and deep-cold treated at a temperature of -180℃ for 2~3 hours.
[0062] After half an hour of deep freezing treatment, the steel is tempered at 550°C for 130 minutes. The tempering treatment is repeated three times, and the steel is air-cooled to room temperature after each tempering.
[0063] S2, semi-finishing the plunger workpiece after tempering, especially fine grinding the working surface of the plunger workpiece.
[0064] S3, nitriding treatment, forming a nitrided layer on the surface of the plunger workpiece at a preset position.
[0065] First, clean the semi-finished plunger workpiece. Then place the semi-finished plunger workpiece as the cathode in a nitriding furnace containing a nitrogen medium. Then raise the temperature in the nitriding furnace to 560°C and keep it warm. At the same time, introduce the nitrogen-containing medium at a rate of 0.7~1L / min, maintain the furnace pressure at (300±20)Pa, and keep it warm for 1600min. After the nitriding is completed, introduce nitrogen to maintain positive pressure, turn on the blower, cool the furnace to 100°C or below, and air cool it to room temperature after it is taken out of the furnace.
[0066] S4, after the nitriding is out of the furnace, the machine is turned for fine grinding, and then the plunger workpiece is cleaned on an ultrasonic cleaning line. Then it is clamped and loaded into the furnace, and then etched for 28 minutes. Then the coating is deposited by plasma enhanced chemical vapor deposition (PECVDPlasma Enhanced Chemical Vapor Deposition) to form a DLC coating on the nitriding layer. Finally, polishing is performed.
[0067] The surface hardness of the workpiece is tested with a nano hardness tester, the hardness of the nitride layer, the depth of the nitride layer and the core hardness are tested with HV1, the bonding force is tested with an indentation method, the coating thickness is tested with a ball pit tester, the grain size is tested with a metallographic microscope, and the friction coefficient is tested with a friction coefficient tester.
[0068] The test results are as follows: After the W6Mo5Cr4V2 dual-fuel engine plunger workpiece is treated by the above method, the hardness at 0.05mm of the base can reach about 1020HV1, and the surface hardness is about 2010HV. The depth of the nitriding layer is 0.10-0.20mm, the hardness of the base core can reach about 780HV1, and the grain size of the base core can reach more than level 11. The thickness of the DLC coating is 1.5μm, the bonding force between the DLC coating and the nitriding layer is HF2-3, and the surface friction coefficient of the DLC coating is about 0.15.
[0069] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.
Claims
1. A plunger processing method, characterized in that: The steps include: S1, heating, heat preservation, quenching, deep cryogenic treatment and tempering are performed on the rough-machined plunger workpiece in sequence; S2, semi-finishing the plunger workpiece after tempering; S3, nitriding treatment, forming a nitrided layer on the surface of the plunger workpiece at a preset position; S4, forming a DLC coating on the nitride layer.
2. The plunger processing method according to claim 1, characterized in that: The heating and heat preservation in S1 include: firstly heating the rough-machined plunger workpiece to 850±10°C and keeping it warm for 20-30 minutes, then heating it to 900±10°C and keeping it warm for 60-90 minutes, and finally heating it to 1180±10°C and keeping it warm for 20-25 minutes.
3. The plunger processing method according to claim 1, characterized in that: The quenching in S1 is vacuum quenching, water quenching or oil quenching.
4. The plunger processing method according to claim 3, characterized in that: The quenching in S1 is vacuum gas quenching, which specifically includes: placing the roughly processed plunger workpiece in a heating furnace, drawing a vacuum, and then heating and keeping it warm. After the insulation is completed, quenching is performed using 2-5 bar nitrogen, and quenching is performed to 60° C. or below before being taken out of the furnace.
5. The plunger processing method according to claim 1, characterized in that: The tempering times in S1 are at least three times, the tempering temperature is 560±10° C., and the tempering time is 120-150 min.
6. The plunger processing method according to claim 1, characterized in that: The nitriding treatment in S3 includes: placing the semi-finished plunger workpiece as a cathode in a nitriding furnace containing a nitrogen medium, then raising the temperature in the nitriding furnace to 560±10°C and keeping it warm, while introducing the nitrogen-containing medium at a rate of 0.7~1L / min, maintaining the furnace pressure at 300±20Pa, and keeping it warm for 1500~1800min; After nitriding is completed, nitrogen is introduced to maintain positive pressure, the furnace is cooled to 100°C or below, and then air-cooled to room temperature after being taken out of the furnace.
7. The plunger processing method according to claim 1, characterized in that: A DLC coating is formed on the nitride layer by using a plasma enhanced chemical vapor deposition method.
8. The plunger processing method according to claim 1, characterized in that: Before S4, the plunger workpiece after nitriding is finely ground, cleaned, and etched.
9. The plunger processing method according to claim 1, characterized in that: After the DLC coating is formed, the plunger workpiece is polished.
10. The plunger processing method according to claim 1, characterized in that: The material grade of the plunger workpiece in S1 is W6Mo5Cr4V2.
Citation Information
Patent Citations
Stacking composite coating piston ring and manufacturing method thereof
CN102777281A
Compressor 38CrMoAl steel treatment technology
CN104911607A
Vacuum step gas quenching method of D6AC ultra-high strength steel thin-walled shell
CN109055683A
Thermal treatment method of Cr12Mo1V1 steel, and application of Cr12Mo1V1 steel
CN109825681A
Application of new nitrided steel in manufacturing of diesel engine plunger and barrel assembly
CN112593156A