Wood sponge-based underwater micro-force sensor and preparation method and application thereof
Through the wood sponge-based underwater microforce sensor without packaging, the micro-nano porous structure and superhydrophobic coating of wood sponge are used to solve the problems of reduced sensitivity and high cost in underwater environments, and the range of 8 meters of water depth is achieved The stable monitoring within the country has expanded the application scope of ocean detection.
Patent Information
- Application Number
- CN202411092346.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Traditional flexible stress sensors have reduced sensitivity after packaging in underwater environments and are costly, making them difficult to be suitable for marine detection.
Using a wood sponge-based underwater microforce sensor without packaging, a micro-nano porous network structure is prepared through wood processing, and a superhydrophobic coating is applied on its surface and inside, using water conductivity and liquid-gas interface movement to transmit electrical signals to avoid conduction agent load.
It has achieved the improvement of sensor sensitivity and application range at low cost, and can stably monitor microforce changes within a water depth of 8 meters, expanding the monitoring range and data real-time performance of ocean detection.
Smart Images

Figure CN118990705A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sensors, and in particular relates to a wood-based sensor and a preparation method and application thereof. Background Art
[0002] As land resources become increasingly scarce, people have gradually turned their attention to the development and utilization of marine resources. However, due to the complex and changeable underwater environment and inconvenient communication conditions, traditional monitoring methods are no longer applicable to the field of marine exploration. Therefore, the underwater monitoring system based on flexible stress sensors has played a great role, effectively expanding the monitoring range and improving the real-time nature of data. It is of great significance in the development and utilization of water resources, prevention and control of water pollution, and marine scientific research.
[0003] When flexible stress sensors are used in underwater environments, they are usually packaged, but packaging will inevitably reduce the sensing sensitivity. For example, pressure changes as low as 0.005Pa in the air can be captured, but the most advanced piezoelectric sensors underwater can only distinguish pressure changes of 10Pa. In addition, flexible stress sensors in the existing technology generally have the disadvantage of being expensive. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a low-cost wood sponge-based underwater micro-force sensor that does not require packaging and a preparation method and application thereof.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A wood sponge-based underwater micro-force sensor comprises a wood sponge and conductive sheets arranged on the upper and lower surfaces of the wood sponge. The wood sponge is a micro-nano porous network structure obtained by processing wood, and the surface and pores of the micro-nano porous network structure are loaded with a super-hydrophobic coating.
[0007] The wood sponge-based underwater micro-force sensor of the present invention does not require packaging or loading of conductive agents. It uses the conductivity of water to establish a current path and uses the movement of the underwater liquid-gas interface to transmit electrical signals (air stored in the micro-nano porous network structure), which is completely different from existing conventional stress sensors.
[0008] As a general technical concept, the present invention also provides a method for preparing the above-mentioned wood sponge-based underwater micro-force sensor, comprising the following steps:
[0009] (1) treating wood with delignification and hemicellulose to obtain delignified wood;
[0010] (2) converting the delignified wood obtained in step (1) into a wood sponge by TEMPO oxidation treatment;
[0011] (3) subjecting the wood sponge obtained in step (2) to super-hydrophobic modification to obtain a super-hydrophobic modified wood sponge;
[0012] (4) Using silver glue, one end of the two copper foils is respectively pasted to the upper and lower surfaces of the super-hydrophobic wood sponge obtained in step (3), thereby obtaining a wood sponge-based underwater micro-force sensor.
[0013] In the above-mentioned preparation method, preferably, the wood sponge obtained in step (2) is subjected to TEMPO oxidation treatment again, and the cellulose nanofiber dispersion is obtained by grinding and shearing dispersion; the wood sponge obtained in step (2) is then impregnated into the above-mentioned cellulose nanofiber dispersion, after vacuum impregnation, freeze-dried, and then steps (3) and (4) are performed. The above-mentioned steps can be used to modify the pore structure inside the wood sponge, extend the underwater three-phase line length for the subsequent super-hydrophobic wood sponge, improve the anti-infiltration property, and act together with the subsequent super-hydrophobic coating, so that the super-hydrophobic effect is better. In addition, the cellulose nanofiber dispersion of the present invention is derived from the wood sponge and is subjected to TEMPO oxidation treatment, grinding and shearing dispersion again, and the cellulose nanofiber dispersion and the wood sponge to be loaded have homology, and the modification effect will be better.
[0014] In the above-mentioned preparation method, preferably, nano silicon dioxide is added to the cellulose nanofiber dispersion, and through ultrasonic dispersion treatment, the mass concentration of the nano silicon dioxide in the cellulose nanofiber dispersion is 0.1-0.3wt%. After the nano silicon dioxide is dispersed in the cellulose nanofiber dispersion, it is conducive to the uniform loading of the nano silicon dioxide. Adding nano silicon dioxide can improve hydrophobicity on the one hand, and provide in-situ growth sites when it is conducive to subsequent super-hydrophobic coating loading on the other hand, and improve the coating loading effect. Meanwhile, in order to ensure that each substance in the cellulose nanofiber dispersion is evenly dispersed, a dispersant can also be added, and the specific dispersant type can be unlimited. Too much nano silicon dioxide addition will result in poor dispersibility, and too little addition will have limited effect.
[0015] In the above preparation method, preferably, when the wood sponge obtained in step (2) is impregnated into the cellulose nanofiber dispersion for vacuum impregnation, the impregnation time is 5-15 min, and the concentration of the cellulose nanofiber dispersion is 0.3-0.7 mg / mL. Continuous stirring can be performed during vacuum impregnation. The concentration of the cellulose nanofiber dispersion needs to be reasonably controlled. If the amount is too small, the modification effect on the inside of the wood sponge is poor, and the hydrophobicity of the wood sponge will be affected. If the amount is too large, the pore structure inside the wood sponge is too small or too small, which will affect the use of the sensor.
[0016] In the above preparation method, preferably, when the wood sponge is subjected to TEMPO oxidation treatment again, the oxidation treatment conditions in step (2) are repeated until the delignified wood tends to be dispersed; the grinding and shearing dispersion is performed by shearing with a disc grinder to disperse it into a cellulose nanofiber dispersion, the rotation speed of the disc grinder is 1500-2000rpm, and it is repeated multiple times, such as 3 times.
[0017] In the above preparation method, preferably, step (1) comprises the following steps: immersing the wood in a mixed aqueous solution of sodium hydroxide and sodium sulfite and boiling it, then immersing it in a hydrogen peroxide solution, heating it in a water bath, taking it out and washing it, and freeze-drying it to obtain delignified wood; controlling the concentration of sodium hydroxide to 2-3 mol / L, the concentration of sodium sulfite to 0.2-0.5 mol / L, the boiling time to 1-3 h, the concentration of hydrogen peroxide solution to 2-3 mol / L, the heating temperature of water bath heating to 70-80°C, and the freeze-drying conditions to freeze at -50 to -40°C for 10-14 h, and then vacuum drying for 45-50 h.
[0018] In the above preparation method, preferably, the oxidizing solution during TEMPO oxidation treatment is a sodium phosphate aqueous solution, and the pH value of the sodium phosphate aqueous solution is adjusted to 6.5-7.0 by using acetic acid, TEMPO and sodium chlorite are added to the sodium phosphate aqueous solution, and the concentration of TEMPO is controlled to be 0.1-0.3 mol / L, and the concentration of sodium chlorite is controlled to be 0.1-0.2 mol / L; at the same time, a mixed aqueous solution of sodium hypochlorite and sodium acetate is added to the sodium phosphate aqueous solution, and the volume ratio of the mixed aqueous solution of sodium hypochlorite and sodium acetate to the sodium phosphate aqueous solution is 1:8-12, and in the mixed aqueous solution of sodium hypochlorite and sodium acetate, the concentration of sodium hypochlorite is 0.1-0.2 mol / L, and the concentration of sodium acetate is 0.1-0.3 mol / L. After the mixed aqueous solution of sodium hypochlorite and sodium acetate and the sodium phosphate aqueous solution are mixed, they are placed at room temperature and away from light for 10-14 hours.
[0019] In the above preparation method, preferably, during the TEMPO oxidation treatment, the reaction temperature is controlled to be 60°C, the reaction time is 48 hours, and after the reaction is completed, freeze drying and then vacuum drying are performed. The freeze drying is performed by freezing at -50°C for 12 hours and then vacuum drying for 48 hours.
[0020] In the above preparation method, preferably, in step (3), when the wood sponge is subjected to super-hydrophobic modification treatment, the wood sponge is immersed in a n-hexane solution of silica and PDMS, vacuum impregnated, and taken out and dried to obtain a super-hydrophobic modified wood sponge; the mass concentration of PDMS in the n-hexane solution is 1.2-1.8wt%, the mass concentration of silica in the n-hexane solution is 0.4-0.6wt%, the immersion time during vacuum impregnation is 5-15min, and the drying temperature during drying is 70-90°C.
[0021] In the above preparation method, preferably, the copper foil is adhered to the upper and lower radial sections of the super-hydrophobic wood sponge using silver glue.
[0022] In the above preparation method, preferably, the width of the copper foil can be 1 cm, the length is not less than the water depth where the sensor is located, and the wood is balsa wood (light wood).
[0023] As a general technical concept, the present invention also provides an application of a wood sponge-based underwater micro-force sensor in underwater real-time monitoring. The wood sponge-based underwater micro-force sensor can be applied to the field of ocean detection, effectively expanding the monitoring range and improving the real-time nature of data, and is of great significance in the development and utilization of water resources, prevention and control of water environment pollution, and marine scientific research.
[0024] More specifically, the method for preparing the wood sponge-based underwater micro-force sensor of the present invention may include the following steps:
[0025] (1) The wood is immersed in a mixed aqueous solution of sodium hydroxide and sodium sulfite and boiled, and after sufficient reaction, washed in water until neutral;
[0026] (2) immersing the wood treated in step (1) in a hydrogen peroxide solution, heating it in a water bath, taking it out, washing it, and freeze-drying it to obtain delignified wood;
[0027] (3) preparing a sodium phosphate aqueous solution with a pH value of 6.5-7.0, adding a mixed aqueous solution of TEMPO, sodium sulfite, sodium hypochlorite and sodium acetate to the solution, mixing and then allowing to stand;
[0028] (4) placing the delignified wood prepared in step (2) into the mixed solution prepared in step (3) to carry out a full oxidation reaction;
[0029] (5) taking out the delignified wood after the reaction in step (4) and immersing it in ethanol, washing it to neutrality, taking it out and freeze-drying it to obtain a wood cellulose matrix;
[0030] (6) placing the delignified wood after the oxidation reaction in step (4) into the mixed solution prepared in step (3) again for reaction until the wood cellulose tends to decompose, taking out and washing to neutrality to obtain a fiber aggregate;
[0031] (7) immersing the fiber aggregate prepared in step (6) in deionized water, shearing it using a disc grinder, and dispersing it into a cellulose nanofiber dispersion (nano-silicon dioxide may be optionally added thereto);
[0032] (8) impregnating the wood cellulose matrix obtained in step (5) in the cellulose nanofiber dispersion prepared in step (7), vacuum impregnating, taking out and freeze-drying to obtain a wood sponge;
[0033] (9) immersing the wood sponge obtained in step (8) in a n-hexane solution of silica and PDMS, vacuum impregnating, taking out and drying to obtain a superhydrophobic modified wood sponge;
[0034] (10) Using silver glue, one end of two copper foils is respectively pasted on the upper and lower surfaces of the superhydrophobic modified wood sponge obtained in step (9) to obtain a wood sponge-based underwater micro-force sensor.
[0035] As a natural renewable resource, wood has become a popular biomass material due to its excellent high strength-to-weight ratio, good environmental properties and processability. The use of wood as a matrix to prepare flexible stress sensors has the characteristics of low cost. Therefore, wood-based flexible stress sensors have good application prospects. However, wood is insulating. Using it in the field of sensors usually requires impregnation with conductive nanomaterials such as graphene, MXene, and carbon nanotubes to construct a conductive network. The preparation process of such conductive nanomaterials is complex and costly. In addition, the liquid-gas interface of the wood-based superhydrophobic structure is prone to failure under high hydrostatic pressure, which limits the underwater application depth range of wood-based flexible stress sensors.
[0036] Based on this, the present invention uses low-cost wood as a matrix to prepare a flexible stress sensor. The elastic wood sponge obtained by structure and component regulation has anisotropic mechanical properties, can withstand high hydrostatic pressure after super-hydrophobic treatment, and a large number of micrometer and nanometer pore structures inside provide space for capturing and storing air, providing a structural basis for preventing air from escaping under high hydrostatic pressure. The nanocellulose loaded on the cell wall surface can further improve the material's anti-infiltration property by increasing the length of the three-phase line. Therefore, the improved wood of the present invention has unique structural characteristics and mechanical characteristics for underwater micro-force sensing.
[0037] Specifically, in the present invention, sodium hydroxide, sodium sulfite and hydrogen peroxide can remove lignin and hemicellulose in wood, and make the wood into delignified wood; during TEMPO oxidation treatment, a sodium phosphate mixed aqueous solution added with a mixed aqueous solution of TEMPO, sodium sulfite, sodium hypochlorite and sodium acetate can separate the cell wall into a microfibril nano-network structure through the electrostatic repulsion between carboxyl groups, and make the delignified wood into a high-elastic wood cellulose matrix with good support; the high-elastic wood cellulose matrix can be prepared into a cellulose nanofiber dispersion by further TEMPO oxidation, grinding and shear dispersion; when the wood cellulose matrix and the cellulose nanofiber dispersion are mixed and impregnated, the cellulose nanofibers can construct a wood cellulose network in the wood cellulose matrix, modify the inside of the wood cellulose matrix, extend the underwater three-phase line length for the subsequent super-hydrophobic wood sponge, and improve the anti-infiltration property; in the preferred scheme, nano-silicon dioxide is also added to the cellulose nanofiber dispersion, which can improve the hydrophobic effect on the one hand, and is conducive to the loading of the subsequent hydrophobic coating on the other hand, as a precursor substance of the hydrophobic coating, to improve the hydrophobic effect. Finally, through super-hydrophobic modification, PDMS and silica as surface modifiers of wood sponge sensing materials are evenly dispersed on the surface of the sensing material, thereby reducing the surface energy to construct a super-hydrophobic surface. The super-hydrophobic strategy makes the sensing material free from encapsulation and preserves air underwater. After the above treatment, the wood sponge has a large number of micron and nano-scale pore structures inside, which provide space for capturing and storing air. The wood sponge has a super-hydrophobic structure and strong anti-infiltration properties. When the wood sponge is placed underwater, the air inside it will not escape. The underwater air layer can be used as a pneumatic spring to ultra-sensitively capture micro-force changes such as micro-vibrations, giving the sensing material ultra-high spatial resolution.
[0038] Compared with the prior art, the advantages of the present invention are:
[0039] 1. The wood sponge-based sensing material of the present invention is different from conventional stress sensors. It does not require conductive nanomaterial loading or packaging. It changes the underwater current propagation path, uses the conductivity of water to establish a current path, and uses the movement of the underwater liquid-gas interface to transmit electrical signals. The air layer stored in the wood sponge acts as a pneumatic spring to ultra-sensitively capture micro-force changes, giving the sensing material an ultra-high spatial resolution. The overall preparation process is simple, the cost is low, and the sensitivity is high.
[0040] 2. The present invention utilizes the anisotropic structure and micrometer- and nanometer-scale pore structure of wood sponge to improve the stability of the liquid-gas interface of the sensing material, so that its underwater air layer can exist stably and is not easily invalidated under high hydrostatic pressure, thereby creating conditions for achieving high-sensitivity and stable underwater sensing, and increasing the application depth range of underwater superhydrophobic mechanical sensing materials from 1.8m to 8m.
[0041] 3. The present invention uses modification to make wood into an underwater micro-force sensor that does not require conductive treatment, which greatly improves the use value of wood, broadens the application scope of wood, and provides support for the monitoring and exploration of marine resources.
[0042] In general, the method for preparing the wood sponge-based underwater micro-force sensor provided by the present invention is simple to operate, has low material cost, does not require packaging, utilizes the underwater liquid-gas interface for electrical signal response, does not require conductive coating loading on the wood sponge, and has low preparation cost. The anisotropic structure of the wood sponge can give the material higher sensitivity and a wider range of water depth application, providing ideas for the high-value utilization of wood in the field of underwater sensing. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0044] Figure 1 This is a comparison chart of the Fourier infrared transmittance of balsa wood, wood sponge and superhydrophobic wood sponge in Example 2.
[0045] Figure 2 This is a graph of 100 repeated compression stresses of the superhydrophobic wood sponge prepared in Example 2.
[0046] Figure 3 Compression-release photos of the superhydrophobic wood sponge prepared in Example 2 (from left to right: before compression, during compression, and after compression).
[0047] Figure 4 This is a comparison diagram of the contact angles of the superhydrophobic wood sponges prepared in Example 1, Example 2, and Example 3.
[0048] Figure 5 This is a photo of the underwater sensing application of the wood sponge-based underwater micro-force sensor prepared in Example 1.
[0049] Figure 6 This is a graph showing the change in water level sensing resistance of the wood sponge-based underwater micro-force sensor prepared in Example 1.
[0050] Figure 7 This is a graph of underwater micro-vibration induced resistance change of the wood sponge-based underwater micro-force sensor prepared in Example 1.
[0051] Figure 8 This is a diagram of the resistance response signal of the wood sponge-based underwater micro-force sensor prepared in Example 1 for different underwater micro-vibrations. DETAILED DESCRIPTION
[0052] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0053] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0054] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0055] Embodiment 1:
[0056] A method for preparing a wood sponge-based underwater micro-force sensor comprises the following steps:
[0057] (1) Delignified wood preparation:
[0058] Use a band saw to cut the balsa wood into 12mm slices, and use a blade to remove the saw marks on the surface. Cut the balsa wood into 10×10×10mm small cubes along the cross section parallel to the wood rays. Wash the balsa wood blocks with deionized water and place them in a ventilated environment to wait for air drying. Use alkali solution delignification method to prepare 2.5mol / L sodium hydroxide and 0.4mol / L sodium sulfite aqueous solution. Immerse the balsa wood blocks in the mixed aqueous solution and boil them for 48h to remove lignin and hemicellulose. The wood blocks with lignin and hemicellulose partially removed are washed several times in deionized water to wash away the internal chemicals. Then immerse them in a hydrogen peroxide solution with a concentration of 2.5mol / L and boil them at 75℃ for 2h to remove lignin and hemicellulose again. Repeatedly wash the residual chemicals and agents. The balsa wood blocks with lignin and hemicellulose removed are placed in the cold trap of the freeze dryer and frozen at -50℃ for 12h. After taking it out, quickly put it into the upper layer of the freeze dryer and vacuum dry it for 48 hours to obtain delignified wood.
[0059] (2) Preparation of highly elastic wood cellulose matrix and wood sponge:
[0060] Prepare 2L of sodium phosphate aqueous solution with a concentration of 0.1mol / L, add acetic acid dropwise to make the pH of the sodium phosphate aqueous solution 6.8. Add TEMPO with a concentration of 0.2mol / L and sodium chlorite with a concentration of 0.125mol / L to the sodium phosphate aqueous solution. Prepare 200mL of a mixed aqueous solution of sodium hypochlorite and sodium acetate, with a sodium hypochlorite concentration of 0.1mol / L and a sodium acetate concentration of 0.2mol / L, add 200mL of a mixed aqueous solution of sodium hypochlorite and sodium acetate to a mixed aqueous solution of sodium phosphate containing TEMPO and sodium chlorite, and place the mixed solution at room temperature and away from light for 12 hours. Immerse the delignified wood in the mixed solution, react at 60°C for 48 hours, take it out and immerse it in ethanol, then wash it to neutrality, take it out and put it in a freeze dryer cold trap, and freeze it at -50°C for 12 hours. After taking it out, quickly put it in the upper layer of the freeze dryer, and vacuum dry it for 48 hours to obtain a wood fiber cellulose matrix.
[0061] The wood cellulose matrix was subjected to TEMPO oxidation treatment again, and then ground and sheared to obtain a cellulose nanofiber dispersion with a concentration of 0.4 mg / mL. The wood cellulose matrix was then immersed in the cellulose nanofiber dispersion, vacuum immersed for 10 minutes, and then taken out and placed in a freeze dryer cold trap, frozen at -50°C for 12 hours. After being taken out, it was quickly placed in the upper layer of the freeze dryer, and vacuum dried for 48 hours to obtain a wood sponge.
[0062] (3) Construction of super-hydrophobic surface of wood sponge:
[0063] Weigh 1.5g PDMS and 0.5g silica, dissolve them in 100g n-hexane and stir evenly. Take a wood sponge sample and immerse it in the prepared silica / PDMS n-hexane solution, and put it into a vacuum device for vacuum impregnation so that the wood sponge can fully load silica and PDMS. After the wood sponge is soaked in the mixed solution for 10 minutes, take out the sample, gently squeeze to remove the excess solution, and then put the sample into a forced air drying oven and dry it at 80°C to obtain a superhydrophobic wood sponge.
[0064] (4) Assembly of underwater micro-force sensor:
[0065] Apply conductive silver paint evenly on the two radial sections of the conductive wood sponge, connect the two ends with 1 cm wide strips cut from high-purity copper foil to reduce the influence of resistance, and connect the end of the copper foil to the digital source meter probe. For fixation, the device connected to the sample can be pasted on a glass slide to reduce data fluctuations caused by sample swing during the test.
[0066] Embodiment 2:
[0067] A method for preparing a wood sponge-based underwater micro-force sensor comprises the following steps:
[0068] (1) Delignified wood preparation:
[0069] Use a band saw to cut the balsa wood into 12mm slices, and use a blade to remove the saw marks on the surface. Cut the balsa wood into 10×10×10mm small cubes along the cross section parallel to the wood rays. Wash the balsa wood blocks with deionized water and place them in a ventilated environment to wait for air drying. Use alkali solution delignification method to prepare 2.5mol / L sodium hydroxide and 0.4mol / L sodium sulfite aqueous solution. Immerse the balsa wood blocks in the mixed aqueous solution and boil them for 48h to remove lignin and hemicellulose. The wood blocks with lignin and hemicellulose partially removed are washed several times in deionized water to wash away the internal chemicals. Then immerse them in a hydrogen peroxide solution with a concentration of 2.5mol / L and boil them at 75℃ for 2h to remove lignin and hemicellulose again. Repeatedly wash the residual chemicals and agents. The balsa wood blocks with lignin and hemicellulose removed are placed in the cold trap of the freeze dryer and frozen at -50℃ for 12h. After taking it out, quickly put it into the upper layer of the freeze dryer and vacuum dry it for 48 hours to obtain delignified wood.
[0070] (2) Preparation of highly elastic wood cellulose matrix and wood sponge:
[0071] Prepare 2L of sodium phosphate aqueous solution with a concentration of 0.1mol / L, add acetic acid dropwise to make the pH of the sodium phosphate aqueous solution 6.8. Add TEMPO with a concentration of 0.2mol / L and sodium chlorite with a concentration of 0.125mol / L to the sodium phosphate aqueous solution. Prepare 200mL of a mixed aqueous solution of sodium hypochlorite and sodium acetate, with a sodium hypochlorite concentration of 0.1mol / L and a sodium acetate concentration of 0.2mol / L, add 200mL of a mixed aqueous solution of sodium hypochlorite and sodium acetate to a mixed aqueous solution of sodium phosphate containing TEMPO and sodium chlorite, and place the mixed solution at room temperature and away from light for 12 hours. Immerse the delignified wood in the mixed solution, react at 60°C for 48 hours, take it out and immerse it in ethanol, then wash it to neutrality, take it out and put it in a freeze dryer cold trap, and freeze it at -50°C for 12 hours. After taking it out, quickly put it in the upper layer of the freeze dryer, and vacuum dry it for 48 hours to obtain a wood fiber cellulose matrix.
[0072] The wood cellulose matrix was subjected to TEMPO oxidation treatment again, and then ground and sheared to obtain a cellulose nanofiber dispersion with a concentration of 0.4 mg / mL. Nano-silicon dioxide was then added to the cellulose nanofiber dispersion, and then ultrasonically dispersed. The mass concentration of nano-silicon dioxide was 0.2 wt%. The wood cellulose matrix was then immersed in the cellulose nanofiber dispersion, and after vacuum immersion for 10 minutes, it was taken out and placed in a freeze dryer cold trap, and frozen at -50°C for 12 hours. After being taken out, it was quickly placed in the upper layer of the freeze dryer, and vacuum dried for 48 hours to obtain a wood sponge.
[0073] (3) Construction of super-hydrophobic surface of wood sponge:
[0074] Weigh 1.5g PDMS and 0.5g silica, dissolve them in 100g n-hexane and stir evenly. Take a wood sponge sample and immerse it in the prepared silica / PDMS n-hexane solution, and put it into a vacuum device for vacuum impregnation so that the wood sponge can fully load silica and PDMS. After the wood sponge is soaked in the mixed solution for 10 minutes, take out the sample, gently squeeze to remove the excess solution, and then put the sample into a forced air drying oven and dry it at 80°C to obtain a superhydrophobic wood sponge.
[0075] (4) Assembly of underwater micro-force sensor:
[0076] Apply conductive silver paint evenly on the two radial sections of the conductive wood sponge, connect the two ends with 1 cm wide strips cut from high-purity copper foil to reduce the influence of resistance, and connect the end of the copper foil to the digital source meter probe. For fixation, the device connected to the sample can be pasted on a glass slide to reduce data fluctuations caused by sample swing during the test.
[0077] The Fourier infrared transmittance comparison of balsa wood, wood sponge and super hydrophobic wood sponge in this embodiment is shown in the figure below. Figure 1 As shown in the figure, it can be seen that wood and hemicellulose are successfully removed, and silica and PDMS are successfully loaded.
[0078] The 100-times repeated compression stress diagram of the super hydrophobic wood sponge prepared in this example is shown in FIG. Figure 2 The results show that the wood sponge can still show good high recovery ability after repeated compression, and has excellent fatigue resistance when used for sensing. The compression-release photos of the superhydrophobic wood sponge prepared in this example are shown in FIG. Figure 3 As shown in the figure, it can be seen that the wood sponge can recover to its shape before compression after compression.
[0079] Embodiment 3:
[0080] A method for preparing a wood sponge-based underwater micro-force sensor comprises the following steps:
[0081] (1) Delignified wood preparation:
[0082] Use a band saw to cut the balsa wood into 12mm slices, and use a blade to remove the saw marks on the surface. Cut the balsa wood into 10×10×10mm small cubes along the cross section parallel to the wood rays. Wash the balsa wood blocks with deionized water and place them in a ventilated environment to wait for air drying. Use alkali solution delignification method to prepare 2.5mol / L sodium hydroxide and 0.4mol / L sodium sulfite aqueous solution. Immerse the balsa wood blocks in the mixed aqueous solution and boil them for 48h to remove lignin and hemicellulose. The wood blocks with lignin and hemicellulose partially removed are washed several times in deionized water to wash away the internal chemicals. Then immerse them in a hydrogen peroxide solution with a concentration of 2.5mol / L and boil them at 75℃ for 2h to remove lignin and hemicellulose again. Repeatedly wash the residual chemicals and agents. The balsa wood blocks with lignin and hemicellulose removed are placed in the cold trap of the freeze dryer and frozen at -50℃ for 12h. After taking it out, quickly put it into the upper layer of the freeze dryer and vacuum dry it for 48 hours to obtain delignified wood.
[0083] (2) Preparation of wood sponge:
[0084] Prepare 2L of sodium phosphate aqueous solution with a concentration of 0.1mol / L, add acetic acid dropwise to make the pH of the sodium phosphate aqueous solution 6.8. Add TEMPO with a concentration of 0.2mol / L and sodium chlorite with a concentration of 0.125mol / L to the sodium phosphate aqueous solution. Prepare 200mL of a mixed aqueous solution of sodium hypochlorite and sodium acetate, with a sodium hypochlorite concentration of 0.1mol / L and a sodium acetate concentration of 0.2mol / L, add 200mL of a mixed aqueous solution of sodium hypochlorite and sodium acetate to a mixed aqueous solution of sodium phosphate containing TEMPO and sodium chlorite, and place the mixed solution at room temperature and away from light for 12 hours. Immerse the delignified wood in the mixed solution, react at 60℃ for 48 hours, take it out and immerse it in ethanol, then wash it to neutrality, take it out and put it in a freeze dryer cold trap, and freeze it at -50℃ for 12 hours. After taking it out, quickly put it in the upper layer of the freeze dryer, and vacuum dry it for 48 hours to obtain a wood sponge.
[0085] (3) Construction of super-hydrophobic surface of wood sponge:
[0086] Weigh 1.5g PDMS and 0.5g silica, dissolve them in 100g n-hexane and stir evenly. Take a wood sponge sample and immerse it in the prepared silica / PDMS n-hexane solution, and put it into a vacuum device for vacuum impregnation so that the wood sponge can fully load silica and PDMS. After the wood sponge is soaked in the mixed solution for 10 minutes, take out the sample, gently squeeze to remove the excess solution, and then put the sample into a forced air drying oven and dry it at 80°C to obtain a superhydrophobic wood sponge.
[0087] (4) Assembly of underwater micro-force sensor:
[0088] Apply conductive silver paint evenly on the two radial sections of the conductive wood sponge, connect the two ends with 1 cm wide strips cut from high-purity copper foil to reduce the influence of resistance, and connect the end of the copper foil to the digital source meter probe. For fixation, the device connected to the sample can be pasted on a glass slide to reduce data fluctuations caused by sample swing during the test.
[0089] The contact angle test was performed on the super hydrophobic wood sponges prepared in Example 1, Example 2, and Example 3. The results are as follows: Figure 4 As shown in the figure, it can be seen that the contact angles of Example 1 and Example 2 are significantly larger. In Example 2, cellulose nanofiber dispersion containing nano-silica is used for impregnation, and the contact angle is larger and the hydrophobic performance is better.
[0090] The underwater sensing application photo of the wood sponge-based underwater micro-force sensor prepared in Example 1 is shown in FIG. Figure 5 As shown, the application status of the wood sponge-based underwater micro-force sensor is demonstrated. The hydrophobicity of the wood sponge makes it have an obvious silver mirror phenomenon underwater, indicating that the air layer around the wood sponge exists stably underwater.
[0091] Use silver glue to stick one end of two copper foils with a width of 1 cm on the upper and lower surfaces of the super-hydrophobic wood sponge sensor material, and connect them to a digital source meter. The digital source meter outputs a constant voltage of 2V and records the resistance change curve of the sensor device.
[0092] The water level sensing resistance change diagram of the wood sponge-based underwater micro-force sensor prepared in Example 1 is as follows Figure 6 As shown, the wood sponge-based underwater micro-force sensor is placed in a sealed water container, and then pressurized by a pressurizing device to simulate a water depth of 0 to 8 meters by adding hydraulic pressure. As can be seen from the figure, the wood sponge-based underwater micro-force sensor can accurately monitor the water level within a wide water pressure range of 0-8m.
[0093] The underwater micro-vibration induced resistance change diagram of the wood sponge-based underwater micro-force sensor prepared in Example 1 is as follows Figure 7 As shown, the wood sponge-based underwater micro-force sensor is placed in a sealed water container, which is placed on a table. A heavy object is used to hit the table. The table transmits the vibration to the container to simulate underwater micro-vibration. It can be seen from the figure that the wood sponge-based underwater micro-force sensor has repeatability and stability for monitoring underwater micro-vibration.
[0094] The resistance response signal diagram of the wood sponge-based underwater micro-force sensor prepared in Example 1 for different underwater micro-vibrations. Figure 8 (b)), knocking on the container wall ( Figure 8 (c)), ultrasonic vibration ( Figure 8 As shown in (d)), blowing ( Figure 8 As shown in (e), stirring ( Figure 8 The underwater micro-vibration caused by the wood sponge-based underwater micro-force sensor (as shown in (f)) shows different resistance response signals, indicating that it is accurate in sensing underwater micro-vibrations.
Claims
1. A wood sponge-based underwater micro-force sensor, characterized in that: The invention comprises a wood sponge and conductive sheets arranged on the upper and lower surfaces of the wood sponge. The wood sponge is a micro-nano porous network structure obtained by processing wood. The surface and pores of the micro-nano porous network structure are loaded with a super-hydrophobic coating.
2. A method for preparing a wood sponge-based underwater micro-force sensor as claimed in claim 1, characterized in that: The following steps are involved: (1) treating wood with delignification and hemicellulose to obtain delignified wood; (2) converting the delignified wood obtained in step (1) into a wood sponge by TEMPO oxidation treatment; (3) subjecting the wood sponge obtained in step (2) to super-hydrophobic modification to obtain a super-hydrophobic modified wood sponge; (4) Using silver glue, one end of the two copper foils is respectively pasted to the upper and lower surfaces of the super-hydrophobic wood sponge obtained in step (3), thereby obtaining a wood sponge-based underwater micro-force sensor.
3. The preparation method according to claim 1, characterized in that: The wood sponge obtained in step (2) is subjected to TEMPO oxidation treatment again, and then ground, sheared and dispersed to obtain a cellulose nanofiber dispersion; the wood sponge obtained in step (2) is then impregnated into the above cellulose nanofiber dispersion, vacuum impregnated, freeze-dried, and then steps (3) and (4) are performed.
4. The preparation method according to claim 3, characterized in that: Nano-silicon dioxide is added into the cellulose nano-fiber dispersion and is subjected to ultrasonic dispersion treatment. The mass concentration of the nano-silicon dioxide in the cellulose nano-fiber dispersion is 0.1-0.3 wt %.
5. The preparation method according to claim 3, characterized in that: When the wood sponge obtained in step (2) is impregnated into the cellulose nanofiber dispersion for vacuum impregnation, the impregnation time is 5-15 minutes, and the concentration of the cellulose nanofiber dispersion is 0.3-0.7 mg / mL.
6. The preparation method according to claim 2, characterized in that: When the wood sponge is subjected to TEMPO oxidation treatment again, the oxidation treatment conditions in step (2) are repeated until the delignified wood tends to be dispersed; the grinding and shearing dispersion is performed by shearing with a disc grinder to disperse it into a cellulose nanofiber dispersion liquid, the rotation speed of the disc grinder is 1500-2000rpm, and it is repeated multiple times.
7. The preparation method according to claim 2, characterized in that: The step (1) comprises the following steps: immersing the wood in a mixed aqueous solution of sodium hydroxide and sodium sulfite and boiling it, then immersing it in a hydrogen peroxide solution, heating it in a water bath, taking it out and washing it, and freeze-drying it to obtain delignified wood; the concentration of sodium hydroxide is controlled to be 2-3 mol / L, the concentration of sodium sulfite is controlled to be 0.2-0.5 mol / L, the boiling time is controlled to be 1-3 hours, the concentration of the hydrogen peroxide solution is controlled to be 2-3 mol / L, the heating temperature of the water bath is controlled to be 70-80°C, and the freeze-drying conditions are freezing at -50 to -40°C for 10-14 hours, and then vacuum drying for 45-50 hours.
8. The preparation method according to claim 2, characterized in that: The oxidation solution during TEMPO oxidation treatment is a sodium phosphate aqueous solution, and acetic acid is used to adjust the pH value of the sodium phosphate aqueous solution to 6.5-7.
0. TEMPO and sodium chlorite are added to the sodium phosphate aqueous solution, and the concentration of TEMPO is controlled to be 0.1-0.3 mol / L, and the concentration of sodium chlorite is controlled to be 0.1-0.2 mol / L. At the same time, a mixed aqueous solution of sodium hypochlorite and sodium acetate is added to the sodium phosphate aqueous solution, and the volume ratio of the mixed aqueous solution of sodium hypochlorite and sodium acetate to the sodium phosphate aqueous solution is 1:8-12. In the mixed aqueous solution of sodium hypochlorite and sodium acetate, the concentration of sodium hypochlorite is 0.1-0.2 mol / L, and the concentration of sodium acetate is 0.1-0.3 mol / L. After the mixed aqueous solution of sodium hypochlorite and sodium acetate and the sodium phosphate aqueous solution are mixed, they are placed at room temperature and away from light for 10-14 hours.
9. The preparation method according to claim 2, characterized in that: In step (3), when the wood sponge is subjected to super-hydrophobic modification, the wood sponge is immersed in a n-hexane solution of silicon dioxide and PDMS, vacuum impregnated, and taken out and dried to obtain a super-hydrophobic modified wood sponge; The mass concentration of PDMS in the n-hexane solution is 1.2-1.8 wt %, the mass concentration of silicon dioxide in the n-hexane solution is 0.4-0.6 wt %, the immersion time during vacuum immersion is 5-15 min, and the drying temperature during drying is 70-90° C.
10. Use of the wood sponge-based underwater micro-force sensor described in claim 1 or the wood sponge-based underwater micro-force sensor prepared by the preparation method according to any one of claims 2 to 9 in underwater real-time monitoring.
Citation Information
Patent Citations
System and method for more efficient automatic irrigation based on a large number of cheap humidity sensors and automatic faucets
CA2446843A1
Novel automatically-controlled wood drying kiln
CN102654351A
Environment-friendly solvent spraying glue and preparation method thereof
CN102775955A
Object detection by whirling system
CN105143819A
Floating substrates including carbonaceous coatings for offshore cultivation of target products and methods of making and using the same
WO2023183913A1
Cited By
Wood-based energy storage building material capable of self-adapting to environment temperature and preparation method of wood-based energy storage building material
CN120382535A
Super-hydrophobic wood-based optical oxygen sensing material as well as preparation method and application thereof
CN121105156A