Preparation method of flame-retardant composite board with clean and efficient utilization of straw fibers

Through the hot pressing forming technology of surface-modified straw fibers and inorganic powders, combined with epoxy resin adhesive, composite boards with good flame retardant and moisture-proof performance are prepared, which solves the problems of flammability and resource waste of wooden boards, and realizes the realization of Efficient utilization of straw and the production of environmentally friendly decorative materials.

CN118991208AActive Publication Date: 2024-11-22SHAANXI SCI TECH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411250239.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Traditional wooden decorative boards are flammable, have poor moisture resistance, high resource consumption, and insufficient utilization of crop straw, resulting in safety hazards, environmental pollution and waste of resources.

Method used

The heat-pressing technology of surface-modified straw fibers and inorganic powder is prepared by combining epoxy resin adhesives and organic resin adhesives to prepare flame-retardant composite boards, which have good thermal insulation performance, fire-proof moisture-proof, dimensional stability and Degradability.

Benefits of technology

It realizes efficient utilization of straw fiber, reduces forest resource consumption, improves the flame retardant performance, physical and mechanical properties and environmental protection of the board, and forms green and safe building decorative materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032042540000121
    Figure BDA0005032042540000121
  • Figure BDA0005032042540000131
    Figure BDA0005032042540000131
  • Figure BDA0005032042540000132
    Figure BDA0005032042540000132
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to a preparation method of a flame-retardant composite board with clean and efficient utilization of straw fibers. The method comprises the following steps: uniformly stirring surface modified straw fibers and surface modified inorganic powder to obtain a mixture; and putting the mixture into a self-made mold, putting the mold into a press vulcanizer, and carrying out hot press molding to obtain the straw fiber-based plate. Uniformly coating the surface of the straw fiber-based plate with an epoxy resin adhesive, and paving facing paper; uniformly coating the epoxy resin adhesive on the surface of the facing paper, and paving the wear-resistant layer; and putting the base plate paved with the facing paper and the wear-resistant layer into a press vulcanizer, and carrying out hot-pressing curing to obtain the flame-retardant composite plate. The board prepared by the method has the performance advantages of being excellent in performance, green, free of formaldehyde, fireproof, moisture-proof and the like, and the board efficiently utilizes the crop straws and is degradable in the natural environment, so that cyclic utilization of agricultural resources is realized, and consumption of forest resources in a decoration industry chain is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a method for preparing a flame-retardant composite board for clean and efficient utilization of straw fibers. Background Art

[0002] With the rapid development of the modern home decoration industry, people's requirements for decorative materials are increasing day by day, especially their concerns about safety, durability and environmental protection have increased significantly. Although traditional wooden decorative panels have certain advantages in terms of aesthetics and processability, their inherent defects are becoming increasingly prominent.

[0003] First of all, the flammability of wood decorative panels is an issue that cannot be ignored. In daily life, areas such as kitchens and bathrooms often require the use of open flames or face high humidity environments, which greatly increases the risk of fire in wood panels. Especially when fire prevention measures are not in place, once the fire source contacts the wood board, the fire will spread rapidly, posing a serious threat to family safety.

[0004] Secondly, wooden decorative panels have poor moisture resistance. In a high humidity environment, such as the rainy season in the south or the humid climate in coastal areas, wooden panels easily absorb moisture, causing mold, deformation and other problems. This not only seriously affects the aesthetics of the decorative effect, but may also breed harmful substances such as bacteria and mold, pollute the indoor air quality, and threaten the health of the residents.

[0005] Thirdly, as the main raw material of traditional decorative panels, excessive consumption of wood has become a problem that cannot be ignored. As people's requirements for the aesthetics of their living environment increase, the use of wooden decorative panels has increased dramatically, which has directly led to the rapid consumption of forest resources.

[0006] Finally, the clean and efficient use of crop straw is also an issue that needs to be urgently addressed. Summary of the invention

[0007] In order to overcome the shortcomings of the above-mentioned prior art and solve the problem of recycling of natural resources, the purpose of the present invention is to provide a method for preparing a flame-retardant composite board that cleanly and efficiently utilizes straw fiber. The board prepared by this method has the advantages of excellent thermal insulation performance, green zero formaldehyde, fire and moisture resistance, good dimensional stability, and the board can be degraded and returned to farmland. After coating or covering the surface decorative layer, it can form various building thermal insulation decorative boards.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing a flame-retardant composite plate for clean and efficient utilization of straw fibers, comprising the following steps:

[0010] The surface-modified straw fiber and the surface-modified inorganic powder are uniformly stirred to obtain a mixture; the mixture is loaded into a self-made mold, the mold is placed in a flat vulcanizer, and the straw fiber-based board is obtained after hot pressing; the epoxy resin adhesive is uniformly applied to the surface of the straw fiber-based board, and a facing paper is laid; the epoxy resin adhesive is uniformly applied to the surface of the facing paper, and a wear-resistant layer is laid; the base board with the facing paper and the wear-resistant layer is placed in a flat vulcanizer, and the flame-retardant composite board is obtained after hot pressing and curing.

[0011] Preferably, the preparation method of the surface-modified straw fiber is: dissolving an organic resin binder in anhydrous ethanol to form an organic resin solution; spraying the organic resin solution evenly on the surface of the heat-modified straw fiber under stirring, and obtaining the surface-modified straw fiber after drying; wherein, in the preparation method of the surface-modified straw fiber, the mass ratio of the heat-modified straw fiber and the organic resin binder is 100:(12-15).

[0012] Preferably, the method for preparing the heat-modified straw fiber is: washing and drying the crop straw, crushing it into fiber powder and then heating it to obtain the heat-modified straw fiber.

[0013] Preferably, the preparation method of the surface-modified inorganic powder is: fly ash, magnesium hydroxide and calcium chloride are mixed evenly to obtain inorganic powder, and an organic resin binder and a silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution; under stirring, the mixed solution is evenly sprayed on the surface of the inorganic powder, and the surface-modified inorganic powder is obtained after sufficient drying; the mass ratio of the fly ash, magnesium hydroxide, calcium chloride, synthetic organic resin binder and silane coupling agent is 100: (30-35): (30-35): (8-10); (2-3).

[0014] Preferably, the preparation method of the organic resin adhesive is: hexamethylenediamine and aminopropyltriethoxysilane are respectively configured as 30% to 35% ethanol solutions; adipic acid and ethanol are mixed, heated and stirred to dissolve the adipic acid, and the hexamethylenediamine solution is added and stirred continuously; the reaction temperature is lowered to room temperature and then the aminopropyltriethoxysilane solution is added, and the reaction is stirred continuously to obtain an organic resin adhesive containing siloxane end groups; wherein the mass ratio of adipic acid, hexamethylenediamine and aminopropyltriethoxysilane is 100:(23-25):(150-160).

[0015] Preferably, the preparation method of the epoxy resin adhesive is: dissolving epoxy resin in benzyl alcohol, adding diethylenetriamine and stirring well to obtain the epoxy resin adhesive.

[0016] Preferably, the mass ratio of the epoxy resin, benzyl alcohol and diethylenetriamine is 10:1:1.

[0017] Preferably, the mass ratio of the surface modified straw fiber to the surface modified inorganic powder is (1.2-1.4):1.

[0018] Preferably, the hot pressing molding is performed under the conditions of 120° C. and 20 MPa for 60 to 90 minutes.

[0019] Preferably, the conditions for hot pressing curing are: hot pressing for 10 minutes at 60° C. and 5-8 MPa, and then standing and curing for 2-3 days after taking out.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The product of the present invention uses crop straw as the main raw material to prepare the base board, which not only provides a new way to process agricultural straw and promotes agricultural income in disguise, but also greatly reduces the consumption of forest resources in the decoration industry chain and promotes the recycling of resources in the decoration industry. The straw fiber in the flame-retardant composite board of the present invention accounts for more than 50%, has a low density and low thermal conductivity, and has the outstanding advantages of light weight and good thermal insulation; the amount of organic resin adhesive used in the straw fiber-based board is small, and the combustion performance of the thermally modified straw fiber is reduced. At the same time, fly ash, magnesium hydroxide and calcium chloride are used as the flame retardant system, and its flame retardant performance reaches Class A.

[0022] Furthermore, the base material of the present invention adopts straw fiber with a high filling ratio, and its physical and mechanical properties and flame retardant properties are enhanced through thermal modification treatment and beneficial compounding of organic resin adhesive and inorganic powder. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0024] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0025] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0026] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0027] The present invention provides a method for preparing a flame-retardant composite board for clean and efficient utilization of straw fibers, which specifically comprises the following steps:

[0028] Thermal modification of straw fiber:

[0029] The crop straw is washed and dried, crushed into fiber powder less than 5 mm by a pulverizer, and the fiber powder is heated at 110-130°C for 24 hours to obtain heat-modified straw fiber; preferably, rice straw, wheat straw and corn straw are used. The crop straw can also be replaced by reed stalks, tree branches and sawdust. The straw fiber is simply heated and modified, which does not require expensive equipment and complex modification processes, and effectively removes excess moisture, impurities and flammable components in the straw fiber.

[0030] Synthesis of organic resin adhesive:

[0031] 1) According to the mass percentage, 100 parts of adipic acid, 23 parts to 25 parts of hexamethylenediamine and 150 parts to 160 parts of aminopropyltriethoxysilane are weighed respectively, and the hexamethylenediamine and aminopropyltriethoxysilane are dissolved in ethanol to form a 30-35% solution.

[0032] 2) Add adipic acid and an appropriate amount of ethanol into a flask, and allow the adipic acid to fully dissolve at 60-100°C with stirring.

[0033] 3) Maintaining the temperature of 60-100°C and stirring, drip the hexamethylenediamine solution into the flask at a rate of 1-2 drops per second, and continue stirring to react for 1-3 hours.

[0034] 4) The reaction temperature is lowered to room temperature, and the aminopropyltriethoxysilane solution is slowly dripped into the above flask under rapid stirring conditions, and the stirring reaction is continued for 2-6 hours to obtain an organic resin adhesive containing siloxane end groups.

[0035] The organic resin adhesive synthesized in the present invention has a simple synthesis process and low cost. Its average relative molecular mass is not high and its viscosity is low, but its siloxane end group has strong adhesion to both straw fiber and inorganic powder. In addition, the organic resin adhesive can be rapidly degraded in the soil, ensuring that the product of the present invention is green and environmentally friendly throughout its life cycle.

[0036] Surface modification of straw fibers:

[0037] According to the mass percentage, 100 parts of the above-mentioned heat-modified straw fiber and 12 to 15 parts of the organic resin adhesive are weighed respectively. The organic resin adhesive is dissolved in anhydrous ethanol to form an organic resin solution with a concentration of 20% to 30%. Under stirring, the organic resin solution is evenly sprayed on the surface of the straw fiber and fully dried at 60-100°C to obtain surface-modified straw fiber. The appropriate amount of synthetic organic resin ensures that the materials have strong adhesion and also ensures that the base material has excellent flame retardant properties.

[0038] Surface modification of inorganic powders

[0039] According to the mass percentage, 100 parts of fly ash, 30 parts to 35 parts of magnesium hydroxide, 30 parts to 35 parts of calcium chloride, 8 parts to 10 parts of organic resin binder and 2 parts to 3 parts of silane coupling agent are weighed respectively. Fly ash, magnesium hydroxide and calcium chloride are mixed evenly to obtain inorganic powder, and organic resin and silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution with a concentration of 25% to 35%. Under stirring, the mixed solution of organic resin binder and silane coupling agent is evenly sprayed on the surface of inorganic powder, and fully dried at 60-100°C to obtain surface-modified inorganic powder. The appropriate amount of synthetic organic resin binder ensures that the materials have strong adhesion and also ensures that the base material has excellent flame retardant properties.

[0040] Hot pressing of straw fiber-based boards:

[0041] According to the mass percentage of (1.2-1.4):1, the surface modified straw fiber and the surface modified inorganic powder are uniformly stirred. The mixed material is loaded into a self-made mold, the mold is placed in a flat vulcanizer, and hot-pressed for 60-90 minutes at 120-160°C and 20-50MPa to obtain a straw fiber-based board. The present invention determines the temperature and pressure of the hot pressing molding of the base board through a large number of experiments, which not only ensures the effective molding of the base board, but also does not cause thermal decomposition of the synthetic organic resin, and at the same time makes the molding of the base board have lower energy consumption.

[0042] Surface film of straw fiber-based board:

[0043] According to the mass percentage of 10:1:1, epoxy resin, benzyl alcohol and ethylenediamine are weighed respectively (ethylenediamine, the raw material of adhesive, can be replaced by polyamines such as diethylenetriamine and triethylenetetramine). Epoxy resin is dissolved in benzyl alcohol, diethylenetriamine is added and stirred thoroughly to obtain epoxy resin adhesive. Then, the epoxy resin adhesive is evenly applied to the surface of the above-mentioned straw fiber-based board, and the facing paper is laid; then, the epoxy resin adhesive is evenly applied to the surface of the facing paper, and the wear-resistant layer is laid; the base board with the facing paper and the wear-resistant layer is placed in a flat vulcanizer, hot-pressed at 60-80°C and 5-8MPa for 10-30min, taken out and left to stand for curing for 2-3d to obtain the flame-retardant composite board. Among them, light-curing resin can also be used instead of epoxy resin adhesive; straw fiber-based board can be flexibly matched with various facing papers and wear-resistant layers to form architectural decorative boards with different decorative styles, such as using colored facing paper and PET wear-resistant layers. The present invention adopts an appropriately proportioned epoxy resin adhesive and a heat curing temperature to ensure that the facing paper and the wear-resistant layer are firmly attached to the surface of the straw fiber-based board.

[0044] The present invention achieves flame retardancy of the base board by adding a certain proportion of inorganic powders such as calcium chloride and magnesium hydroxide to the straw fiber; at the same time, in order to make the organic straw fiber and the inorganic powder have a strong bonding force and improve the moisture-proof ability of the base board, the present invention uses a directional synthesized organic resin to perform organic-inorganic hybrid modification on the material. In the composite process of the straw fiber, the organic synthetic resin and the inorganic powder, the moisture content and other undesirable components of the straw fiber will have a great impact on the organic-inorganic hybrid modification. Too high a moisture content will lead to defects such as voids and stress inside the base board, while the straw fiber in a completely dry state is relatively brittle, and the shear stress of the molding process will cut the fiber; at the same time, the straw fiber may also have some undesirable components that affect its surface grafting modification. Therefore, the present invention performs a thermal modification treatment on the straw fiber to remove excess moisture and other volatile undesirable components. The temperature and time need to be well controlled for thermal modification of straw fiber: if the temperature is too low or the time is insufficient, these components cannot be fully removed; if it is overheated or the time is too long, the hemicellulose in the straw fiber will be thermally degraded and the lignin will be thermally rearranged, which will seriously affect the performance of the straw fiber-based board. The present invention optimizes the heating temperature and time of the straw fiber through a large number of experiments, removes the volatile substances in the straw fiber in a controllable manner, regulates the surface properties of the straw fiber, and thus improves the physical and mechanical properties and surface chemical properties of the straw fiber material.

[0045] The adhesive used in the base board of the present invention is a directional synthetic resin with zero formaldehyde content, which can be fully degraded in a natural soil environment in a relatively short time. Waste base boards can be returned to farmland as fertilizer, thus achieving green environmental protection throughout the life cycle of building decorative boards.

[0046] The temperature required for hot pressing of the base plate and hot bonding of the surface decorative layer and the wear-resistant layer of the product of the present invention is relatively low, the energy consumption in the production process is low, and it has outstanding energy-saving and environmental protection advantages; and the production process of the product of the present invention is relatively simple, suitable for large-scale production, and has strong adaptability to promotion.

[0047] Example 1

[0048] The rice straw is washed and dried, and then crushed into fiber powder less than 5 mm by a pulverizer, and the fiber powder is heated at 110°C for 24 hours to obtain heat-modified straw fiber; 100 parts of adipic acid, 23 parts of hexamethylenediamine and 150 parts of aminopropyltriethoxysilane are weighed according to mass percentage, and hexamethylenediamine and aminopropyltriethoxysilane are respectively configured into 30% ethanol solution.

[0049] Add adipic acid and an appropriate amount of ethanol to a flask, and fully dissolve the adipic acid at 60°C with stirring. Keep the temperature at 60°C and stirring, drip the hexamethylenediamine solution into the flask at a rate of 1 drop per second, and continue stirring to react for 3 hours. Lower the reaction temperature to room temperature, and slowly drip the aminopropyltriethoxysilane solution into the flask under rapid stirring, and continue stirring to react for 2 hours to obtain an organic resin adhesive containing siloxane end groups.

[0050] According to the mass percentage, 100 parts of the above-mentioned heat-modified straw fiber and 12 parts of the organic resin binder are weighed respectively. The organic resin binder is dissolved in anhydrous ethanol to form an organic resin solution with a concentration of 20%. Under stirring, the organic resin solution is evenly sprayed on the surface of the straw fiber, and fully dried at 60° C. to obtain surface-modified straw fiber.

[0051] According to the mass percentage, 100 parts of fly ash, 30 parts of magnesium hydroxide, 30 parts of calcium chloride, 9 parts of organic resin binder and 2 parts of silane coupling agent are weighed respectively. The fly ash, magnesium hydroxide and calcium chloride are mixed evenly, and the organic resin and silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution with a concentration of 25%. Under stirring, the mixed solution of organic resin binder and silane coupling agent is evenly sprayed on the surface of inorganic powder, and fully dried at 60°C to obtain surface-modified inorganic powder.

[0052] According to the mass percentage, 1.2 parts of surface-modified straw fiber and 1 part of surface-modified inorganic powder were mixed evenly. The mixture was put into a self-made mold, and the mold was placed in a flat vulcanizer, and hot-pressed for 90 minutes at 120°C and 20MPa to obtain a straw fiber-based board.

[0053] According to the mass percentage of 10:1:1, epoxy resin, benzyl alcohol and ethylenediamine are weighed respectively. Epoxy resin is dissolved in benzyl alcohol, ethylenediamine is added and stirred thoroughly to obtain epoxy resin adhesive. Then, the epoxy resin adhesive is evenly applied to the surface of the straw fiber-based board and covered with facing paper; then, the epoxy resin adhesive is evenly applied to the surface of the color facing paper and covered with a PET wear-resistant layer; the base board with facing paper and wear-resistant layer is placed in a flat vulcanizer, hot-pressed at 60°C and 5MPa for 30 minutes, and then taken out and cured for 2 days to obtain the flame-retardant composite board.

[0054] Example 2

[0055] The wheat straw is washed and dried, and then crushed into fiber powder less than 5 mm by a pulverizer, and the fiber powder is heated at 120°C for 18 hours to obtain heat-modified straw fiber; 100 parts of adipic acid, 24 parts of hexamethylenediamine and 155 parts of aminopropyltriethoxysilane are weighed according to mass percentage, and hexamethylenediamine and aminopropyltriethoxysilane are respectively configured into 32% ethanol solution.

[0056] Add adipic acid and an appropriate amount of ethanol to a flask, and fully dissolve the adipic acid at 70°C with stirring. Keep the temperature at 70°C and stirring, drip the hexamethylenediamine solution into the flask at a rate of 1 drop per second, and continue stirring to react for 2 hours. Lower the reaction temperature to room temperature, and slowly drip the aminopropyltriethoxysilane solution into the flask under rapid stirring, and continue stirring to react for 3 hours to obtain an organic resin adhesive containing siloxane end groups.

[0057] According to the mass percentage, 100 parts of the above-mentioned heat-modified straw fiber and 12 parts of the organic resin binder are weighed respectively. The organic resin binder is dissolved in anhydrous ethanol to form an organic resin solution with a concentration of 25%. Under stirring, the organic resin solution is evenly sprayed on the surface of the straw fiber, and fully dried at 70°C to obtain surface-modified straw fiber.

[0058] According to the mass percentage, 100 parts of fly ash, 32 parts of magnesium hydroxide, 32 parts of calcium chloride, 9 parts of organic resin binder and 2 parts of silane coupling agent are weighed respectively. The fly ash, magnesium hydroxide and calcium chloride are mixed evenly, and the organic resin and silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution with a concentration of 30%. Under stirring, the mixed solution of organic resin binder and silane coupling agent is evenly sprayed on the surface of inorganic powder, and fully dried at 70°C to obtain surface-modified inorganic powder.

[0059] According to the mass percentage, 1.3 parts of surface-modified straw fiber and 1 part of surface-modified inorganic powder were mixed evenly. The mixture was put into a homemade mold, and the mold was placed in a flat vulcanizer, and hot-pressed for 80 minutes at 130°C and 30MPa to obtain a straw fiber-based board.

[0060] According to the mass percentage of 10:1:1, epoxy resin, benzyl alcohol and diethylenetriamine are weighed respectively. Epoxy resin is dissolved in benzyl alcohol, diethylenetriamine is added and stirred thoroughly to obtain epoxy resin adhesive. Then, the epoxy resin adhesive is evenly applied to the surface of the straw fiber-based board and covered with facing paper; then, the epoxy resin adhesive is evenly applied to the surface of the color facing paper and covered with a PET wear-resistant layer; the base board with facing paper and wear-resistant layer is placed in a flat vulcanizer, hot-pressed at 70°C and 7MPa for 20 minutes, and then taken out and cured for 3 days to obtain the flame-retardant composite board.

[0061] Example 3

[0062] The corn stalks are washed and dried, and then crushed into fiber powder less than 5 mm using a pulverizer, and the fiber powder is heated at 130°C for 12 hours to obtain thermally modified straw fibers; 100 parts of adipic acid, 25 parts of hexamethylenediamine and 160 parts of aminopropyltriethoxysilane are weighed according to mass percentage, and hexamethylenediamine and aminopropyltriethoxysilane are respectively configured into 35% ethanol solutions.

[0063] Add adipic acid and an appropriate amount of ethanol to a flask, and fully dissolve the adipic acid at 80°C under stirring conditions. Keep the temperature at 80°C and stirring conditions, drip the hexamethylenediamine solution into the flask at a rate of 2 drops per second, and continue stirring to react for 1 hour. Lower the reaction temperature to room temperature, and slowly drip the aminopropyltriethoxysilane solution into the flask under rapid stirring conditions, and continue stirring to react for 4 hours to obtain an organic resin adhesive containing siloxane end groups.

[0064] According to the mass percentage, 100 parts of the above-mentioned heat-modified straw fiber and 14 parts of the organic resin binder are weighed respectively. The organic resin binder is dissolved in anhydrous ethanol to form an organic resin solution with a concentration of 30%. Under stirring, the organic resin solution is evenly sprayed on the surface of the straw fiber, and fully dried at 80°C to obtain surface-modified straw fiber.

[0065] According to the mass percentage, 100 parts of fly ash, 35 parts of magnesium hydroxide, 35 parts of calcium chloride, 10 parts of organic resin binder and 3 parts of silane coupling agent are weighed respectively. The fly ash, magnesium hydroxide and calcium chloride are mixed evenly, and the organic resin and silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution with a concentration of 35%. Under stirring, the mixed solution of organic resin binder and silane coupling agent is evenly sprayed on the surface of inorganic powder, and fully dried at 80°C to obtain surface-modified inorganic powder.

[0066] According to the mass percentage, 1.3 parts of surface-modified straw fiber and 1 part of surface-modified inorganic powder were mixed evenly. The mixture was put into a self-made mold, and the mold was placed in a flat vulcanizer, and hot-pressed for 70 minutes at 150°C and 40MPa to obtain a straw fiber-based board.

[0067] According to the mass percentage of 10:1:1, epoxy resin, benzyl alcohol and triethylenetetramine are weighed respectively. Epoxy resin is dissolved in benzyl alcohol, triethylenetetramine is added and stirred thoroughly to obtain epoxy resin adhesive. Then, the epoxy resin adhesive is evenly applied to the surface of the straw fiber-based board and covered with facing paper; then, the epoxy resin adhesive is evenly applied to the surface of the color facing paper and covered with a PET wear-resistant layer; the base board with facing paper and wear-resistant layer is placed in a flat vulcanizer, hot-pressed at 80°C and 8MPa for 10 minutes, and then taken out and cured for 3 days to obtain the flame-retardant composite board.

[0068] Example 4

[0069] The reed stalks are washed and dried, and then crushed into fiber powder less than 5 mm using a pulverizer, and the fiber powder is heated at 130°C for 24 hours to obtain thermally modified straw fibers; 100 parts of adipic acid, 25 parts of hexamethylenediamine and 155 parts of aminopropyltriethoxysilane are weighed according to mass percentage, and hexamethylenediamine and aminopropyltriethoxysilane are respectively configured into 35% ethanol solutions.

[0070] Add adipic acid and an appropriate amount of ethanol to a flask, and fully dissolve the adipic acid at 90°C with stirring. Keep the temperature at 90°C and stirring, drip the hexamethylenediamine solution into the flask at a rate of 2 drops per second, and continue stirring to react for 1 hour. Lower the reaction temperature to room temperature, and slowly drip the aminopropyltriethoxysilane solution into the flask under rapid stirring, and continue stirring to react for 5 hours to obtain an organic resin adhesive containing siloxane end groups.

[0071] According to the mass percentage, 100 parts of the above-mentioned heat-modified straw fiber and 12 parts of the organic resin binder are weighed respectively. The organic resin binder is dissolved in anhydrous ethanol to form an organic resin solution with a concentration of 30%. Under stirring, the organic resin solution is evenly sprayed on the surface of the straw fiber, and fully dried at 90° C. to obtain surface-modified straw fiber.

[0072] According to the mass percentage, 100 parts of fly ash, 30 parts of magnesium hydroxide, 35 parts of calcium chloride, 8 parts of organic resin binder and 2 parts of silane coupling agent are weighed respectively. The fly ash, magnesium hydroxide and calcium chloride are mixed evenly, and the organic resin and silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution with a concentration of 35%. Under stirring, the mixed solution of organic resin binder and silane coupling agent is evenly sprayed on the surface of inorganic powder, and fully dried at 90°C to obtain surface-modified inorganic powder.

[0073] According to the mass percentage, 1.4 parts of surface-modified straw fiber and 1 part of surface-modified inorganic powder were mixed evenly. The mixture was put into a homemade mold, and the mold was placed in a flat vulcanizer, and hot-pressed for 60 minutes at 150°C and 50MPa to obtain a straw fiber-based board.

[0074] According to the mass percentage of 10:1:1, epoxy resin, benzyl alcohol and triethylenetetramine are weighed respectively. Epoxy resin is dissolved in benzyl alcohol, triethylenetetramine is added and stirred thoroughly to obtain epoxy resin adhesive. Then, the epoxy resin adhesive is evenly applied to the surface of the straw fiber-based board and covered with facing paper; then, the epoxy resin adhesive is evenly applied to the surface of the color facing paper and covered with a PET wear-resistant layer; the base board with facing paper and wear-resistant layer is placed in a flat vulcanizer, hot-pressed at 60°C and 8MPa for 10 minutes, and then taken out and cured for 3 days to obtain the flame-retardant composite board.

[0075] Example 5

[0076] The rice straw is washed and dried, and then crushed into fiber powder less than 5 mm by a pulverizer, and the fiber powder is heated at 130°C for 24 hours to obtain heat-modified straw fiber; 100 parts of adipic acid, 23 parts of hexamethylenediamine and 160 parts of aminopropyltriethoxysilane are weighed according to mass percentage, and hexamethylenediamine and aminopropyltriethoxysilane are respectively configured into 35% ethanol solution.

[0077] Add adipic acid and an appropriate amount of ethanol to a flask, and fully dissolve the adipic acid at 100°C with stirring. Keep the temperature at 100°C and stirring, drip the hexamethylenediamine solution into the flask at a rate of 1 drop per second, and continue stirring to react for 1 hour. Lower the reaction temperature to room temperature, and slowly drip the aminopropyltriethoxysilane solution into the flask under rapid stirring, and continue stirring to react for 6 hours to obtain an organic resin adhesive containing siloxane end groups.

[0078] According to the mass percentage, 100 parts of the above-mentioned heat-modified straw fiber and 15 parts of the organic resin binder are weighed respectively. The organic resin binder is dissolved in anhydrous ethanol to form an organic resin solution with a concentration of 30%. Under stirring, the organic resin solution is evenly sprayed on the surface of the straw fiber, and fully dried at 100° C. to obtain surface-modified straw fiber.

[0079] According to the mass percentage, 100 parts of fly ash, 35 parts of magnesium hydroxide, 30 parts of calcium chloride, 10 parts of organic resin binder and 3 parts of silane coupling agent are weighed respectively. Fly ash, magnesium hydroxide and calcium chloride are mixed evenly, and organic resin and silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution with a concentration of 35%. Under stirring, the mixed solution of organic resin binder and silane coupling agent is evenly sprayed on the surface of inorganic powder, and fully dried at 100°C to obtain surface-modified inorganic powder.

[0080] According to the mass percentage, 1.4 parts of surface-modified straw fiber and 1 part of surface-modified inorganic powder were mixed evenly. The mixture was put into a self-made mold, and the mold was placed in a flat vulcanizer, and hot-pressed for 60 minutes at 160°C and 50MPa to obtain a straw fiber-based board.

[0081] According to the mass percentage of 10:1:1, epoxy resin, benzyl alcohol and triethylenetetramine are weighed respectively. Epoxy resin is dissolved in benzyl alcohol, triethylenetetramine is added and stirred thoroughly to obtain epoxy resin adhesive. Then, the epoxy resin adhesive is evenly applied to the surface of the straw fiber-based board and covered with facing paper; then, the epoxy resin adhesive is evenly applied to the surface of the color facing paper and covered with a PET wear-resistant layer; the base board with facing paper and wear-resistant layer is placed in a flat vulcanizer, hot-pressed at 60°C and 8MPa for 10 minutes, and then taken out and cured for 3 days to obtain the flame-retardant composite board.

[0082] The flame retardant composite panels prepared in Examples 1-5 were tested for performance, as shown in Table 1, Table 2 and Table 3:

[0083] Table 1 Surface hardness of flame retardant composite panels prepared in Examples 1-5

[0084]

[0085] As can be seen from Table 1, the hardness of the flame retardant composite board prepared by the present invention is above 60°, and it has strong compression resistance, bending resistance and wear resistance. It can not only effectively resist the physical impact and wear in daily use and extend the service life, but also improve the stability and durability of the overall decoration.

[0086] Table 2 Oxygen index (LOI) of flame retardant composite panels prepared in Examples 1-5

[0087]

[0088] It can be seen from Table 2 that the oxygen index (LOI) of the flame retardant composite board prepared by the present invention is all below 45, and the lowest reaches 31.8, which shows that the present invention has good flame retardant performance.

[0089] Table 3 Impact strength of flame retardant composite panels prepared in Examples 1-5

[0090]

[0091] It can be seen from Table 3 that the impact strength of the flame retardant composite board prepared by the present invention is 5KJ / m 2 Above, the highest reached 9.3KJ / m 2 The high impact strength indicates that the plate prepared by the present invention is not easily damaged or deformed when subjected to a sudden impact, which is crucial for improving the safety and durability of building decoration materials.

[0092] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber, characterized in that: The following steps are involved: The surface-modified straw fiber and the surface-modified inorganic powder are uniformly stirred to obtain a mixture; the mixture is loaded into a self-made mold, the mold is placed in a flat vulcanizer, and the straw fiber-based board is obtained after hot pressing; the epoxy resin adhesive is uniformly applied to the surface of the straw fiber-based board, and a facing paper is laid; the epoxy resin adhesive is uniformly applied to the surface of the facing paper, and a wear-resistant layer is laid; the base board with the facing paper and the wear-resistant layer is placed in a flat vulcanizer, and the flame-retardant composite board is obtained after hot pressing and curing.

2. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 1, characterized in that: The preparation method of the surface-modified straw fiber is as follows: dissolving an organic resin binder in anhydrous ethanol to form an organic resin solution; spraying the organic resin solution uniformly on the surface of the heat-modified straw fiber under stirring, and obtaining the surface-modified straw fiber after drying; wherein, in the preparation method of the surface-modified straw fiber, the mass ratio of the heat-modified straw fiber to the organic resin binder is 100:(12-15).

3. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 2, characterized in that: The method for preparing the heat-modified straw fiber is as follows: the crop straw is washed and dried, crushed into fiber powder, and then heated to react to obtain the heat-modified straw fiber.

4. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 1, characterized in that: The preparation method of the surface-modified inorganic powder is as follows: fly ash, magnesium hydroxide and calcium chloride are uniformly mixed to obtain inorganic powder, and an organic resin binder and a silane coupling agent are dissolved in anhydrous ethanol to form a mixed solution; under stirring, the mixed solution is uniformly sprayed on the surface of the inorganic powder, and the surface-modified inorganic powder is obtained after being fully dried; the mass ratio of the fly ash, magnesium hydroxide, calcium chloride, synthetic organic resin binder and silane coupling agent is 100:(30-35):(30-35):(8-10);(2-3).

5. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 4, characterized in that: The preparation method of the organic resin adhesive is as follows: hexamethylenediamine and aminopropyltriethoxysilane are dissolved in ethanol to prepare a 30% to 35% solution; adipic acid and ethanol are mixed, heated and stirred to dissolve the adipic acid, and the hexamethylenediamine solution is added and stirred continuously; the reaction temperature is lowered to room temperature and then the aminopropyltriethoxysilane solution is added, and the organic resin adhesive containing siloxane end groups is obtained after continuous stirring and reaction; wherein the mass ratio of adipic acid, hexamethylenediamine and aminopropyltriethoxysilane is 100:(23-25):(150-160).

6. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 1, characterized in that: The preparation method of the epoxy resin adhesive comprises the following steps: dissolving epoxy resin in benzyl alcohol, adding diethylenetriamine and stirring the mixture thoroughly to obtain the epoxy resin adhesive.

7. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 6, characterized in that: The mass ratio of the epoxy resin, benzyl alcohol and diethylenetriamine is 10:1:

1.

8. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 1, characterized in that: The mass ratio of the surface modified straw fiber to the surface modified inorganic powder is (1.2-1.4):

1.

9. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 1, characterized in that: The conditions of the hot pressing molding are: hot pressing at 120° C. and 20 MPa for 60 to 90 minutes.

10. The method for preparing a flame-retardant composite board for clean and efficient utilization of straw fiber according to claim 1, characterized in that: The conditions of the hot pressing curing are: hot pressing for 10 minutes at 60° C. and 5-8 MPa, and then standing and curing for 2-3 days after taking out.

Citation Information

Patent Citations

  • Building board combining magnesium compounds and plant fibre and preparation method thereof

    CN101423371A

  • Manufacturing technology of environment-friendly anti-flaming straw board

    CN107127841A

  • Flame-retardant straw-based panel and manufacturing method thereof

    CN108247805A

  • Method for preparing mildew-proof flame-retardant fiber boards

    CN110126054A

  • Straw composite board and manufacturing method thereof

    CN114833912A